DIN 17174 Grade 13MnNi6-3 – Normalized or Normalized Formed (+N) Steel Properties
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.85 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Elongation | 20.0 °C | 22 % | |
Elongation, transverse | 20.0 °C | 20 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Nickel Steel |
Shear modulus | 23.0 °C | 76 GPa | Typical for Nickel Steel |
Tensile strength | 20.0 °C | 490 - 610 MPa | |
Tensile strength, transverse | 20.0 °C | 490 - 610 MPa | |
Yield strength | 20.0 °C | 335 - 355 MPa | |
Yield strength, transverse | 20.0 °C | 335 - 355 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Melting point | 1316 - 1595 °C | Typical for Nickel Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 42.5 W/(m·K) | |
100.0 °C | 43.5 W/(m·K) | ||
200.0 °C | 42.8 W/(m·K) | ||
300.0 °C | 40.9 W/(m·K) | ||
400.0 °C | 39 W/(m·K) | ||
500.0 °C | 36.4 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.7 mm²/s | |
100.0 °C | 11.2 mm²/s | ||
200.0 °C | 10.3 mm²/s | ||
300.0 °C | 9.3 mm²/s | ||
400.0 °C | 8.3 mm²/s | ||
500.0 °C | 7 mm²/s | ||
600.0 °C | 5.7 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.45E-7 Ω·m |
100.0 °C | 2.94E-7 Ω·m | |
200.0 °C | 3.69E-7 Ω·m | |
300.0 °C | 4.59E-7 Ω·m | |
400.0 °C | 5.58E-7 Ω·m | |
500.0 °C | 6.79E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Aluminium | 0.02 % |
Carbon | 0.18 % |
Manganese | 0.85 - 1.65 % |
Nickel | 0.3 - 0.85 % |
Niobium | 0.05 % |
Phosphorus | 0.03 % |
Silicon | 0.5 % |
Sulfur | 0.025 % |
Vanadium | 0.05 % |
Metal
- DIN 2394-2: Grade St 28 Steel – Normalized & Normalized Formed (+N) Properties
- DIN 17174 Grade 11MnNi5-3 – Normalized or Normalized-Formed Steel Specification
- DIN 17173 Grade 13MnNi6-3: Normalized and Normalized‑Formed Steel Specifications
- DIN 17240 Grade C35 Steel – Normalized or Normalized‑Formed (+N) for Creep Resistance up to 400 °C
- DIN 2395‑3 Grade M22 Tubes – Normalized & Normalized‑Formed (N)
- DIN 2391-2: Grade St 30 Al Seamless Steel Tubes – Normalized or Formed (+N)
- DIN 2391‑2 Grade St 30 Si – Normalized or Normalized Formed (N) Steel Tubes for Precision Applications
- DIN 1629 Grade St 52.0 – High‑Strength Normalized Steel Tubes
- DIN 17174: TTSt 35 Normalized/Normalized Formed Steel Specification (+N)
- DIN 17175 Grade St 35.8 Tube Steel – Normalized & Normalized Formed (+N) – High‑Temperature Seamless Tubes