EN 10132-3 Grade C40E Quenched Steel – Premium Cold-Rolled Narrow Strip

Cold-rolled narrow strip made of the mild steel C40E will be delivered in thicknesses up to 6 mm for quenching and tempering in following conditions: - soft annealed or soft annealed and little rerolled (+A or +LC), - cold rolled (+CR). The delivery condition annealed to globular carbides (+AC) can be agreed.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.82 - 7.85 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

217 GPa

20.0 °C

210 - 212 GPa

100.0 °C

205 - 207 GPa

200.0 °C

195 - 199 GPa

300.0 °C

185 - 192 GPa

400.0 °C

175 - 184 GPa

500.0 °C

175 GPa

600.0 °C

164 GPa

Hardness, Rockwell C

20.0 °C

51 [-]

Hardness, Vickers

20.0 °C

530 [-]

Poisson's ratio

23.0 °C

0.29 [-]

Typical for Medium Carbon Steel

Shear modulus

20.0 °C

81 GPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.08E-5 1/K

20.0 °C

1.19E-5 1/K

100.0 °C

1.11E-5 - 1.25E-5 1/K

200.0 °C

1.21E-5 - 1.3E-5 1/K

300.0 °C

1.29E-5 - 1.36E-5 1/K

400.0 °C

1.35E-5 - 1.41E-5 1/K

500.0 °C

1.45E-5 1/K

600.0 °C

1.49E-5 1/K

Max service temperature

500 °C

Typical for Carbon Steel

Melting point

1380 - 1514 °C

Typical for Medium Carbon Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

20.0 °C

461 - 480 J/(kg·K)

100.0 °C

479 - 500 J/(kg·K)

200.0 °C

499 - 550 J/(kg·K)

300.0 °C

517 - 590 J/(kg·K)

400.0 °C

536 J/(kg·K)

500.0 °C

558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Thermal conductivity

20.0 °C

48 - 52 W/(m·K)

100.0 °C

48.9 - 50.6 W/(m·K)

200.0 °C

47.5 - 48.1 W/(m·K)

300.0 °C

44.7 - 45.7 W/(m·K)

400.0 °C

41.6 W/(m·K)

500.0 °C

38.6 W/(m·K)

600.0 °C

35.5 W/(m·K)

Thermal diffusivity

20.0 °C

13.3 mm²/s

100.0 °C

12.6 mm²/s

200.0 °C

11.5 mm²/s

300.0 °C

10.2 mm²/s

400.0 °C

8.9 mm²/s

500.0 °C

7.5 mm²/s

600.0 °C

6 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.2E-7 - 2.17E-7 Ω·m

100.0 °C

2.62E-7 Ω·m

200.0 °C

3.32E-7 Ω·m

300.0 °C

4.2E-7 Ω·m

400.0 °C

5.23E-7 Ω·m

500.0 °C

6.41E-7 Ω·m

600.0 °C

7.8E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.37 - 0.44 %

Chromium

0.4 %

Manganese

0.5 - 0.8 %

Molybdenum

0.1 %

Nickel

0.4 %

Phosphorus

0.04 %

Silicon

0.4 %

Sulfur

0.035 %


Metal

  1. EN 10132-3 Grade 42CrMo4 – Quenched & Tempered Cold Rolled Steel (Up to 6 mm)
  2. EN 10132-3: 42CrMo4 Quenched & Tempered Alloy Steel – Premium Cold-Rolled Strips
  3. EN 10083-2 Grade C40E Quenched Steel for High-Heat Applications
  4. EN 10132-3: 34CrMo4 Alloy Steel – Quenched Grade (Q) for High-Performance Applications
  5. EN 10132-3 25CrMo4 Quenched Steel – Premium Narrow Strip
  6. EN 10132-3 Grade C40E Cold-Rolled Mild Steel – Premium Strip for Quenching & Tempering
  7. EN 10132-3 Grade C45E Quenched – Premium Mild Steel Strip for Precision Rolling
  8. EN 10132-3 Grade C50E Quenched Cold-Rolled Strip – Premium Mild Steel for Advanced Applications
  9. EN 10132-3 Grade C55E Quenched Steel Strip – Specifications & Delivery Conditions
  10. EN 10132-3 Grade C60E Quenched Cold‑Rolled Steel Strip – 0.3 mm to 6 mm