DIN 17440 X4CrMoS18 Soft Annealed Steel – Superior Corrosion Resistance & Versatile Fastener Applications
Properties: - stainless free cutting steel - application in quenched and tempered state - corrosion resistance is similar to an 13%-Cr-steel, because of its sulfur additional - application temperature: -25 to 550 °C Application: - for application enviroment like water, steam, weak alkaline and neutral media - for screws, nuts, fittings, axis, bolts, spindles - for magnetic valve
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.65 - 7.7 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | 20.0 °C | 196 - 216 GPa | |
100.0 °C | 213 GPa | ||
200.0 °C | 207 GPa | ||
300.0 °C | 200 GPa | ||
400.0 °C | 192 GPa | ||
Elongation | 20.0 °C | 20 % | |
Hardness, Brinell | 20.0 °C | 200 [-] | |
Poisson's ratio | 23.0 °C | 0.3 [-] | Typical for Martensitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa | Typical for Martensitic Stainless Steel |
Tensile strength | 20.0 °C | 450 - 650 MPa | |
Yield strength Rp0.2 | 20.0 °C | 270 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 9.2E-6 1/K | |
20.0 °C | 9.9E-6 1/K | ||
100.0 °C | 1E-5 - 1.03E-5 1/K | ||
200.0 °C | 1.05E-5 - 1.08E-5 1/K | ||
300.0 °C | 1.05E-5 - 1.12E-5 1/K | ||
400.0 °C | 1.05E-5 - 1.16E-5 1/K | ||
500.0 °C | 1.1E-5 - 1.19E-5 1/K | ||
600.0 °C | 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K | ||
900.0 °C | 1.34E-5 1/K | ||
1000.0 °C | 1.39E-5 1/K | ||
Melting point | 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Specific heat capacity | 20.0 °C | 450 - 460 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 19.6 - 25 W/(m·K) | |
Thermal diffusivity | 20.0 °C | 5.7 mm²/s | |
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 6.17E-7 - 7E-7 Ω·m |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.06 % |
Chromium | 16.5 - 18.5 % |
Manganese | 1.5 % |
Molybdenum | 0.2 - 0.6 % |
Phosphorus | 0.06 % |
Silicon | 1 % |
Sulfur | 0.15 - 0.35 % |
Metal
- DIN 17440: X6CrMoS17 Soft-Annealed Steel (Grade +A) – Industrial Specification
- DIN 17440 X45CrMoV15 Soft Annealed Steel – High Hardness, Wear Resistance
- DIN 17440 Grade X46Cr13 – Soft Annealed Stainless Steel for Precision Cutting Tools and Wear-Resistant Components
- X17CrNi16-2 Soft Annealed Steel – DIN 17440 Grade for Pressure Vessels & Industrial Applications
- DIN 17440 X12CrMoS17 Soft Annealed Steel – Superior Corrosion Resistance & Versatile Industrial Uses
- DIN 17440 Grade X14CrMoS17 – Soft‑Annealed Stainless Steel for Pressure Vessels & Mechanical Parts
- DIN 17440 Grade X30Cr13 Soft-Annealed Steel – High-Performance Cutting & Bearing Applications
- DIN 17440 Grade X20Cr13 Soft-Annealed Steel (+A): High-Performance Corrosion Resistance & Temperature Stability
- DIN 17440 X6CrTi17 Soft Annealed Steel – Corrosion-Resistant Grade for Industrial Use
- DIN 17440 X6Cr13 Soft-Annealed Alloy – Premium Corrosion & High-Temperature Performance