AW-5083 H18 Aluminum Alloy – EN 573-3 Certified Grade

Naturally hard AlMg alloy. The alloy is food safe.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.66 g/cm³

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

2.64 - 2.66 g/cm³

H18

EN 573-3

Seamless Tube

20.0 °C

2.64 g/cm³

H18

EN 573-3

Seamless Tube

20.0 °C

2.66 g/cm³

H18

EN 573-3

Seamless Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270.0 °C

70.0 GPa

H18

EN 573-3

Seamless Tube

71.0 GPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

70.0 GPa

H18

EN 573-3

Seamless Tube

20.0 °C

70.0 - 71.0 GPa

H18

EN 573-3

Seamless Tube

20.0 °C

71.0 GPa

H18

EN 573-3

Seamless Tube

50.0 °C

69.0 GPa

H18

EN 573-3

Seamless Tube

100.0 °C

68.0 GPa

H18

EN 573-3

Seamless Tube

150.0 °C

66.0 GPa

H18

EN 573-3

Seamless Tube

200.0 °C

63.0 GPa

H18

EN 573-3

Seamless Tube

250.0 °C

57.0 GPa

H18

EN 573-3

Seamless Tube

300.0 °C

50.0 GPa

H18

EN 573-3

Seamless Tube

Elongation

4.0 %

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

A100

20.0 °C

4.0 %

H18

EN 573-3

Seamless Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

H18

EN 573-3

Seamless Tube

Shear modulus

26.8 GPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

26.8 - 27.0 GPa

H18

EN 573-3

Seamless Tube

20.0 °C

26.8 GPa

H18

EN 573-3

Seamless Tube

Tensile strength

-196.0 °C

575.0 MPa

H18

EN 573-3

420.0 MPa

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

420.0 MPa

H18

EN 573-3

Seamless Tube

20.0 °C

445.0 MPa

H18

EN 573-3

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.23e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

-50.0 °C

2.23e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

20 °C

2.23e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

20 °C

2.42e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

20 °C

2.4999999999999998e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20 °C

2.6e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

100 °C

2.42e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

100.0 °C

2.42e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

200 °C

2.4999999999999998e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

200.0 °C

2.5e-05 1/K

H18

EN 573-3

Seamless Tube

300 °C

2.6e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

300.0 °C

2.6e-05 1/K

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

Max service temperature

-195.0 - 50.0 °C

H18

EN 573-3

Seamless Tube

Long

150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

574.0 - 638.0 °C

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Specific heat capacity

900.0 J/(kg·K)

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

899.0 - 900.0 J/(kg·K)

H18

EN 573-3

Seamless Tube

20.0 °C

899.0 J/(kg·K)

H18

EN 573-3

Seamless Tube

20.0 °C

900.0 J/(kg·K)

H18

EN 573-3

Seamless Tube

Thermal conductivity

20.0 °C

110.0 - 140.0 W/(m·K)

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

20.0 °C

110.0 - 117.0 W/(m·K)

H18

EN 573-3

Seamless Tube

20.0 °C

117.0 - 140.0 W/(m·K)

H18

EN 573-3

Seamless Tube

20.0 °C

117.0 W/(m·K)

H18

EN 573-3

Seamless Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

16000000.0 - 19000000.0 S/m

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar, Seamless Tube

Electrical resistivity

5.26e-08 - 6.25e-08 Ω·m

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

20.0 °C

5.2e-08 - 6e-08 Ω·m

H18

EN 573-3

Seamless Tube

20.0 °C

5.2e-08 - 6.2e-08 Ω·m

H18

EN 573-3

Seamless Tube

20.0 °C

6e-08 Ω·m

H18

EN 573-3

Seamless Tube

20.0 °C

6e-08 - 6.2e-08 Ω·m

H18

EN 573-3

Seamless Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.05 - 0.25 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Copper

0.1 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Iron

0.4 %

H18

EN 573-3

Seamless Tube

0.40 %

H18

EN 573-3, EN 1592

Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Magnesium

4.0 - 4.9 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Manganese

0.4 - 1.0 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Silicon

0.4 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Titanium

0.15 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Zinc

0.25 %

H18

EN 573-3, EN 1592

Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / poor, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O)


Metal

  1. EN 573-3 Grade 3.1305 H18 Aluminium Alloy Specifications
  2. AW-8006 H18 – Certified EN 573-3 AlFeMn Alloy: Food Safe, High Strength & Durability
  3. AW-8079 H18 Aluminum Alloy – EN 573-3 Certified, Food‑Safe, High‑Strength
  4. EN 573-3 Grade 3.1325 H18 Aluminium – Key Properties & Standards
  5. EN 573-3 Grade 3.2315 H18 – Aluminum 6000 Series Properties
  6. EN 573-3 Grade 3.3206 H18 – Detailed Material Properties & Standards
  7. AW-2117 H18: Premium Age-Hardenable AlCu Alloy (EN 573-3 Grade)
  8. EN 573-3 Grade AW-6056 H18 – High-Strength Age-Hardenable AlMgSi Alloy
  9. EN 573-3 Grade 3.3555 H18 Aluminium – Technical Overview
  10. EN 573-3 Grade AW-2011 H18 – High-Performance Aluminum Alloy for Precision Machining