The cold-upsettable steel 34 CrNiMo 8 can be cold-formed with the suitable tools with a medium rate of forming according to the usual forming methods on single-stage and multi-stage presses. It is used for high-strength screws of strength class 12.9 in the thick dimension range. For special stress, screws of strength class 14.9 in the thin dimension range can be produced.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.8 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Nickel Chromium Molybdenum Steel |
Reduction of area | 20.0 °C | 58 % | |
Tensile strength | 20.0 °C | 700 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Melting point | 1382 - 1529 °C | Typical for Nickel Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 33.7 W/(m·K) | |
100.0 °C | 36.2 W/(m·K) | ||
200.0 °C | 37.8 W/(m·K) | ||
300.0 °C | 37.2 W/(m·K) | ||
400.0 °C | 35.7 W/(m·K) | ||
500.0 °C | 34 W/(m·K) | ||
600.0 °C | 32 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 9.4 mm²/s | |
100.0 °C | 9.4 mm²/s | ||
200.0 °C | 9.2 mm²/s | ||
300.0 °C | 8.5 mm²/s | ||
400.0 °C | 7.6 mm²/s | ||
500.0 °C | 6.6 mm²/s | ||
600.0 °C | 5.4 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 3.09E-7 Ω·m |
100.0 °C | 3.54E-7 Ω·m | |
200.0 °C | 4.18E-7 Ω·m | |
300.0 °C | 5.05E-7 Ω·m | |
400.0 °C | 6.09E-7 Ω·m | |
500.0 °C | 7.27E-7 Ω·m | |
600.0 °C | 8.67E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.26 - 0.34 % |
Chromium | 1.8 - 2.2 % |
Manganese | 0.3 - 0.6 % |
Molybdenum | 0.3 - 0.5 % |
Nickel | 1.8 - 2.2 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.035 % |
Metal
- EN 10263-4 Grade 41Cr4 – Annealed for Spheroidized Carbides & Precision Turning
- EN 10263-4: Grade 42CrMo4 Steel – Annealed for Spheroidized Carbides and Precision Turning
- EN 10263-4 Grade 46Cr2: Annealed for Spheroidized Carbides & Precision Turning
- EN 10263-4 Grade 34Cr4 Steel – Annealed with Spheroidized Carbides for Hexagonal Screws
- EN 10263-4 Grade 34CrNiMo6 – Annealed for Spheroidized Carbides, Ideal for High‑Strength Screws & Stress‑Critical Extrusions
- EN 10263-4 Grade 37Cr4: Annealed for Spheroidized Carbides and Precision Turning
- EN 10263‑4 Grade 38Cr2 – Annealed for Spheroidized Carbides & Precision Turning
- EN 10263-4 Grade 25CrMo4: Annealed for Spheroidized Carbides & Turned Components
- EN 10263-4 Grade 34CrMo4: Annealed for Spheroidized Carbides and Precision Turning
- EN 10263-4 Grade Cq35 – Annealed Steel with Spheroidized Carbides for High-Strength Screws and Nuts