EN 10277-5 Grade 34CrNiMo6 – Cold Drawn/Turned, Soft Annealed Steel for High-Load Applications
Steel 34 CrNiMo 6 is suitable for high loaded parts (also heavy forged parts) of high heat-treatment sections and favorable ductility qualities in aircraft and heavy-vehicle construction and in machine engineering (e.g. propeller shafts, connecting rods, transmission shafts). Lowest application temp. -40 °C.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.8 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Hardness, Brinell | 20.0 °C | 248 [-] | |
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Nickel Chromium Molybdenum Steel |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Max service temperature, long | -40 - 0 °C | ||
Melting point | 1382 - 1529 °C | Typical for Nickel Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 33.7 W/(m·K) | |
100.0 °C | 36.2 W/(m·K) | ||
200.0 °C | 37.8 W/(m·K) | ||
300.0 °C | 37.2 W/(m·K) | ||
400.0 °C | 35.7 W/(m·K) | ||
500.0 °C | 34 W/(m·K) | ||
600.0 °C | 32 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 9.4 mm²/s | |
100.0 °C | 9.4 mm²/s | ||
200.0 °C | 9.2 mm²/s | ||
300.0 °C | 8.5 mm²/s | ||
400.0 °C | 7.6 mm²/s | ||
500.0 °C | 6.6 mm²/s | ||
600.0 °C | 5.4 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 3.09E-7 Ω·m |
100.0 °C | 3.54E-7 Ω·m | |
200.0 °C | 4.18E-7 Ω·m | |
300.0 °C | 5.05E-7 Ω·m | |
400.0 °C | 6.09E-7 Ω·m | |
500.0 °C | 7.27E-7 Ω·m | |
600.0 °C | 8.67E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.3 - 0.38 % |
Chromium | 1.4 - 1.7 % |
Manganese | 0.4 - 0.7 % |
Molybdenum | 0.15 - 0.3 % |
Nickel | 1.4 - 1.7 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.03 % |
Metal
- 25CrMo4 Steel – EN 10277-5 Cold Drawn, Soft Annealed, High Strength & Ductility
- EN 10277-5 Grade 25CrMoS4 – Cold‑Drawn, Turned & Soft‑Annealed High‑Strength Steel
- EN 10277-5 Grade 38CrS2: Cold Drawn/Turned & Soft Annealed Steel for High-Performance Applications
- EN 10277-5 Grade 41Cr4 – Cold-Drawn, Soft-Annealed Steel for Automotive & Mechanical Use
- EN 10277-5 Grade 41CrS4 Steel – Cold Drawn, Turned & Soft Annealed for Automotive & Industrial Applications
- EN 10277-5 Grade 42CrMo4: Cold Drawn, Turned & Soft Annealed Steel for High-Load Applications
- EN 10277-5 Grade 46Cr2 – Cold‑Drawn or Turned, Soft‑Annealed Steel for Automotive & Machine Applications
- EN 10277-5 Grade 46CrS2: Cold Drawn, Turned & Soft-Annealed Steel for High-Strength Automotive Parts
- EN 10277‑5 Grade 50CrMo4: Cold‑Drawn or Turned, Soft‑Annealed Steel for High‑Load Applications
- EN 10277-5 Grade 50CrV4: High-Performance Cold Drawn or Turned Steel for Heavy-Duty Applications