CuSn6, mat. No. CW425K, is comparable to the DIN-make CuSn6, mat. No. 2.1020, acc. to DIN 17662 : 1983-12. Properties of the CuSn-alloy are predominantly determined by the tin-content. Tensile strength, yield point and hardness increase according to the rising cold forming grade, elongation after fracture decreases. Electrical and thermal conductivity are lower than for pure copper. Very high resistance to corrosion, particularly to atmospheric influences, seawater, sulfite liquor, carbonated and salted mine water. The alloys are stress corrosion-proof. Processing properties: warm forming: medium cold forming: very good machinability: medium hard soldering: good soft soldering: good gas shielded welding: good burnishing: good Appliction: For all types of springs, especially in electrical industry, for connectors, hose and spring tubes, fabric and screening wires, gong bars. Further application in paper, cellulose and chemical industry, in shipbuilding and machine engineering. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.8 - 8.82 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

118 GPa

Elongation

20.0 °C

55 %

Elongation A50

20.0 °C

45 %

Poisson's ratio

20.0 °C

0.34 [-]

Tensile strength

20.0 °C

350 - 420 MPa

Yield strength Rp0.2

20.0 °C

300 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

100.0 °C

1.8E-5 1/K

200.0 °C

1.85E-5 1/K

650.0 °C

2.22E-5 1/K

800.0 °C

2.18E-5 1/K

Specific heat capacity

20.0 °C

377 J/(kg·K)

Thermal conductivity

20.0 °C

75 W/(m·K)

200.0 °C

98 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

9.00E+6 S/m

200.0 °C

7.80E+6 S/m

Electrical resistivity

20.0 °C

1.11E-7 Ω·m

200.0 °C

1.28E-7 Ω·m

Specific Electrical conductivity

16 % IACS

Chemical properties

PropertyValue

Iron

0.1 %

Lead

0.02 %

Nickel

0.2 %

Phosphorus

0.01 - 0.4 %

Tin

5.5 - 7 %

Zinc

0.2 %


Metal

  1. EN 1652 Grade CuSn6 H125 – Premium Tin‑Copper Alloy for Superior Strength and Corrosion Resistance
  2. EN 1652 CuSn6 R720: Premium Tin-Copper Alloy for Superior Corrosion Resistance
  3. EN 1652 Grade CuNi30Mn1Fe R350 – High-Strength, Corrosion-Resistant Copper Alloy
  4. EN 1652 Grade CuSn6 M – Premium Tin-Copper Alloy for Superior Corrosion Resistance
  5. EN 1652 Grade CuSn6 H080 – Premium Tin-Copper Alloy with Enhanced Corrosion Resistance
  6. EN 1652 CuSn6 H180 – High‑Strength Tin‑Copper Alloy for Durable Applications
  7. EN 1652 Grade CuSn6 R560: Premium Tin-Copper Alloy for Industrial Applications
  8. EN 1652 Grade CuSn6 R640 – High-Performance Tin‑Copper Alloy
  9. EN 1652 Grade CuZn37 R350 – Premium Unhardenable Copper Alloy for Cold Forming
  10. EN 1652 Grade CuSn6 R500 – Premium Tin‑Copper Alloy for High‑Performance Applications