EN 10277-5 Grade Ck45 Steel – Cold‑Drawn, Turned & Soft‑Annealed for Heavy‑Duty Applications
Steel CK 45 is suitable for mean strained parts of higher dimensions (heavy forged parts) and complexer forms in vehicle manufacturing and machine engineering (e.g. ship shafts, transmission parts, wheel hubs). Lowest application temp. -25 °C, favorable creep behaviour up to 480 °C.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.8 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Hardness, Brinell | 20.0 °C | 207 [-] | |
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Medium Carbon Steel |
Shear modulus | 23.0 °C | 75 - 80 GPa | Typical for Carbon Steel |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K | ||
Max service temperature | 500 °C | Typical for Carbon Steel | |
Max service temperature, long | -25 - 480 °C | ||
Melting point | 1380 - 1514 °C | Typical for Medium Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41.7 W/(m·K) | |
100.0 °C | 43.4 W/(m·K) | ||
200.0 °C | 43.2 W/(m·K) | ||
300.0 °C | 41.4 W/(m·K) | ||
400.0 °C | 39.1 W/(m·K) | ||
500.0 °C | 36.7 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.6 mm²/s | |
100.0 °C | 11.3 mm²/s | ||
200.0 °C | 10.5 mm²/s | ||
300.0 °C | 9.5 mm²/s | ||
400.0 °C | 8.3 mm²/s | ||
500.0 °C | 7.1 mm²/s | ||
600.0 °C | 5.8 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.5E-7 Ω·m |
100.0 °C | 2.95E-7 Ω·m | |
200.0 °C | 3.65E-7 Ω·m | |
300.0 °C | 4.53E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m | |
500.0 °C | 6.74E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.42 - 0.5 % |
Manganese | 0.5 - 0.8 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.03 % |
Metal
- 25CrMo4 Steel – EN 10277-5 Cold Drawn, Soft Annealed, High Strength & Ductility
- EN 10277-5 Grade 25CrMoS4 – Cold‑Drawn, Turned & Soft‑Annealed High‑Strength Steel
- EN 10277-5 Grade 38CrS2: Cold Drawn/Turned & Soft Annealed Steel for High-Performance Applications
- EN 10277-5 Grade 41Cr4 – Cold-Drawn, Soft-Annealed Steel for Automotive & Mechanical Use
- EN 10277-5 Grade 41CrS4 Steel – Cold Drawn, Turned & Soft Annealed for Automotive & Industrial Applications
- EN 10277-5 Grade 42CrMo4: Cold Drawn, Turned & Soft Annealed Steel for High-Load Applications
- EN 10277-5 Grade 46Cr2 – Cold‑Drawn or Turned, Soft‑Annealed Steel for Automotive & Machine Applications
- EN 10277-5 Grade 46CrS2: Cold Drawn, Turned & Soft-Annealed Steel for High-Strength Automotive Parts