EN 10297-1 Grade 34CrMo4 Quenched & Tempered Steel – Properties & Performance
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.81 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Elongation | 20.0 °C | 11 - 15 % | |
Elongation, transverse | 20.0 °C | 9 - 13 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Chromium Molybdenum Steel |
Reduction of area | 20.0 °C | 45 - 55 % | |
Reduction of area, transverse | 20.0 °C | 45 - 55 % | |
Tensile strength | 20.0 °C | 750 - 1200 MPa | |
Tensile strength, transverse | 20.0 °C | 750 - 1200 MPa | |
Yield strength | 20.0 °C | 500 - 800 MPa | |
Yield strength, transverse | 20.0 °C | 500 - 800 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Melting point | 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 39.6 W/(m·K) | |
100.0 °C | 41.6 W/(m·K) | ||
200.0 °C | 41.8 W/(m·K) | ||
300.0 °C | 40.3 W/(m·K) | ||
400.0 °C | 38.2 W/(m·K) | ||
500.0 °C | 36 W/(m·K) | ||
600.0 °C | 33.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11 mm²/s | |
100.0 °C | 10.8 mm²/s | ||
200.0 °C | 10.1 mm²/s | ||
300.0 °C | 9.2 mm²/s | ||
400.0 °C | 8.1 mm²/s | ||
500.0 °C | 7 mm²/s | ||
600.0 °C | 5.7 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.63E-7 Ω·m |
100.0 °C | 3.08E-7 Ω·m | |
200.0 °C | 3.78E-7 Ω·m | |
300.0 °C | 4.66E-7 Ω·m | |
400.0 °C | 5.69E-7 Ω·m | |
500.0 °C | 6.87E-7 Ω·m | |
600.0 °C | 8.26E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.3 - 0.37 % |
Chromium | 0.9 - 1.2 % |
Manganese | 0.6 - 0.9 % |
Molybdenum | 0.15 - 0.3 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.035 % |
Metal
- Premium 34CrMo4 Cold Rolled Strip – EN 10132‑3 Quenched & Tempered (QT)
- EN 10297-1 Grade 25CrMo4 Quenched & Tempered Steel – Properties & Applications
- EN 10297‑1 Grade 30CrMoV9: Quenched & Tempered Steel (QT) – Key Mechanical & Physical Properties
- EN 10297‑1 Grade 30CrNiMo8 (QT) – Comprehensive Mechanical & Physical Properties
- EN 10297-1 Grade 34CrNiMo6 – Quenched & Tempered Steel: Detailed Mechanical Properties
- EN 10297-1 Grade 41Cr4 Quenched & Tempered Steel – Properties & Performance
- EN 10297-1: Grade 36Mn5 Quenched & Tempered Steel – Specifications & Properties
- EN 10297-1 Grade Cm60 – Quenched & Tempered Steel: High Strength & Reliability
- EN 10263-4 Grade 34CrMo4 Quenched & Tempered Steel – High Strength & Versatility
- EN 10297‑1 Grade 28Mn6 Quenched & Tempered Steel (QT) – Key Mechanical Properties