DIN 17115 Grade USt 35-2 – Normalized or Normalized‑Formed Steel (±N)
The steel is used for welded round link chains and chain components.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.85 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Low Carbon Steel |
Shear modulus | 23.0 °C | 82 GPa | Typical for Low Carbon Steel |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K | ||
Max service temperature | 500 °C | Typical for Carbon Steel | |
Melting point | 1480 - 1526 °C | Typical for Low Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 56.9 W/(m·K) | |
100.0 °C | 56.4 W/(m·K) | ||
200.0 °C | 53.5 W/(m·K) | ||
300.0 °C | 49.4 W/(m·K) | ||
400.0 °C | 45.2 W/(m·K) | ||
500.0 °C | 41.3 W/(m·K) | ||
600.0 °C | 37.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 15.7 mm²/s | |
100.0 °C | 14.5 mm²/s | ||
200.0 °C | 12.9 mm²/s | ||
300.0 °C | 11.2 mm²/s | ||
400.0 °C | 9.6 mm²/s | ||
500.0 °C | 7.9 mm²/s | ||
600.0 °C | 6.3 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 1.83E-7 Ω·m |
100.0 °C | 2.27E-7 Ω·m | |
200.0 °C | 2.95E-7 Ω·m | |
300.0 °C | 3.8E-7 Ω·m | |
400.0 °C | 4.81E-7 Ω·m | |
500.0 °C | 5.99E-7 Ω·m | |
600.0 °C | 7.38E-7 Ω·m | |
Magnetic
| Property | Value | Comment |
|---|---|---|
Curie temperature | 770 °C | Typical for Low Carbon Steel |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.06 - 0.14 % |
Copper | 0.25 % |
Manganese | 0.4 - 0.6 % |
Nitrogen | 0.01 % |
Phosphorus | 0.04 % |
Sulfur | 0.035 % |
Metal
- DIN 2394-2: Grade St 28 Steel – Normalized & Normalized Formed (+N) Properties
- DIN 2394-2: Grade USt 28 – Normalized or Normalized-Formed Steel Specification
- DIN 2394-2 Grade USt 34-2 – Normalized or Normalized Formed (+N) Steel Properties
- DIN 2394-2 Grade USt 37-2: Normalized or Normalized-Formed Steel Standard
- DIN 17240 Grade C35 Steel – Normalized or Normalized‑Formed (+N) for Creep Resistance up to 400 °C
- DIN 17115 21Mn4Al Steel – Normalized or Normalized Formed (+N): Specs & Uses
- DIN 17115 Grade 15Mn3Al Steel – Normalized & Normalized Formed (+N) for Welded Chain Applications
- DIN 17115 RSt 35-2 Grade Steel – Normalized or Normalized Formed (+N) for Chain Applications
- DIN 2395‑3 Grade M22 Tubes – Normalized & Normalized‑Formed (N)
- DIN 2395-3 USt 37-2 Precision Tubes: Normalized/Normalized Formed (±N) – Automotive Grade