EN 10273 Grade 16Mo3 Steel – Normalized or Normalized Formed (+N) for High-Temperature Applications
The steel 16Mo3 is a high temperature steel. Application: pressure vessel and steam boiler construction for vaporizor ducts, ducts, and collector ducts, heat exchangers, welding-neck laps and flanges. Maximum temperature for continuous use: 530 °C.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.85 - 7.86 g/cm³ |
50.0 °C | 7.84 g/cm³ | |
100.0 °C | 7.82 g/cm³ | |
150.0 °C | 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ | |
250.0 °C | 7.77 g/cm³ | |
300.0 °C | 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ | |
450.0 °C | 7.7 g/cm³ | |
500.0 °C | 7.68 g/cm³ | |
550.0 °C | 7.66 g/cm³ | |
600.0 °C | 7.64 g/cm³ | |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa |
20.0 °C | 212 - 212.48 GPa | |
50.0 °C | 211.6 GPa | |
100.0 °C | 207 - 209.25 GPa | |
150.0 °C | 206.11 GPa | |
200.0 °C | 199 - 202.48 GPa | |
250.0 °C | 198.36 GPa | |
300.0 °C | 192 - 194.14 GPa | |
350.0 °C | 189.82 GPa | |
400.0 °C | 184 - 185.51 GPa | |
450.0 °C | 180.99 GPa | |
500.0 °C | 175 - 176.48 GPa | |
550.0 °C | 171.97 GPa | |
600.0 °C | 164 - 166.97 GPa | |
Elongation | 20.0 °C | 19 - 24 % |
Poisson's ratio | 20.0 °C | 0.29 [-] |
50.0 °C | 0.29 [-] | |
100.0 °C | 0.29 [-] | |
150.0 °C | 0.29 [-] | |
200.0 °C | 0.29 [-] | |
250.0 °C | 0.29 [-] | |
300.0 °C | 0.29 [-] | |
350.0 °C | 0.29 [-] | |
400.0 °C | 0.3 [-] | |
450.0 °C | 0.3 [-] | |
500.0 °C | 0.3 [-] | |
550.0 °C | 0.3 [-] | |
600.0 °C | 0.3 [-] | |
Shear modulus | 20.0 °C | 82.6 GPa |
50.0 °C | 82.21 GPa | |
100.0 °C | 81.23 GPa | |
150.0 °C | 79.95 GPa | |
200.0 °C | 78.48 GPa | |
250.0 °C | 76.81 GPa | |
300.0 °C | 75.05 GPa | |
350.0 °C | 73.38 GPa | |
400.0 °C | 71.61 GPa | |
450.0 °C | 69.75 GPa | |
500.0 °C | 67.98 GPa | |
550.0 °C | 66.22 GPa | |
600.0 °C | 64.35 GPa | |
Tensile strength | 20.0 °C | 420 - 590 MPa |
Yield strength | 20.0 °C | 220 - 275 MPa |
Yield strength Rp0.2 | 50.0 °C | 218 - 273 MPa |
100.0 °C | 211 - 264 MPa | |
150.0 °C | 200 - 250 MPa | |
200.0 °C | 186 - 233 MPa | |
250.0 °C | 171 - 213 MPa | |
300.0 °C | 155 - 194 MPa | |
350.0 °C | 140 - 175 MPa | |
400.0 °C | 127 - 159 MPa | |
450.0 °C | 118 - 147 MPa | |
500.0 °C | 113 - 141 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Max service temperature, long | 0 - 530 °C | ||
Melting point | 1382 - 1529 °C | Typical for Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 52.1 W/(m·K) | |
100.0 °C | 51.2 W/(m·K) | ||
200.0 °C | 48.7 W/(m·K) | ||
300.0 °C | 45.5 W/(m·K) | ||
400.0 °C | 42.3 W/(m·K) | ||
500.0 °C | 39.1 W/(m·K) | ||
600.0 °C | 36 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 14.4 mm²/s | |
100.0 °C | 13.2 mm²/s | ||
200.0 °C | 11.7 mm²/s | ||
300.0 °C | 10.3 mm²/s | ||
400.0 °C | 9 mm²/s | ||
500.0 °C | 7.5 mm²/s | ||
600.0 °C | 6 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2E-7 - 2.16E-7 Ω·m |
50.0 °C | 2.37E-7 Ω·m | |
100.0 °C | 2.5E-7 - 2.68E-7 Ω·m | |
150.0 °C | 3.02E-7 Ω·m | |
200.0 °C | 3.24E-7 - 3.39E-7 Ω·m | |
250.0 °C | 3.8E-7 Ω·m | |
300.0 °C | 4.12E-7 - 4.25E-7 Ω·m | |
350.0 °C | 4.74E-7 Ω·m | |
400.0 °C | 5.14E-7 - 5.27E-7 Ω·m | |
450.0 °C | 5.83E-7 Ω·m | |
500.0 °C | 6.33E-7 - 6.42E-7 Ω·m | |
550.0 °C | 7.08E-7 Ω·m | |
600.0 °C | 7.69E-7 - 7.78E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.12 - 0.2 % |
Chromium | 0.3 % |
Copper | 0.3 % |
Manganese | 0.4 - 0.9 % |
Molybdenum | 0.25 - 0.35 % |
Nickel | 0.3 % |
Nitrogen | 0.01 % |
Phosphorus | 0.03 % |
Silicon | 0.35 % |
Sulfur | 0.01 - 0.025 % |
Metal
- EN 10273 Grade P460NH – High-Temperature Normalized Steel for Pressure Vessel Applications
- EN 10222-2 Grade 16Mo3 Steel – Normalized or Normalized Formed (+N) for High‑Temperature Applications
- EN 10217-2 Grade 16Mo3 Normalized Steel Tubes – Ideal for High-Temperature, High-Pressure Applications
- EN 10217‑5: 16Mo3 Steel – Normalized & Normalized Formed (+N) for High‑Temperature Applications
- EN 10216-2 Grade 16Mo3: Normalized or Normalized Formed Tubes for High-Temperature Applications
- EN 10273 Grade P275NH Steel: Normalized or Normalized Formed (+N) – High-Temperature Pressure Vessel Grade
- EN 10273: Grade P355GH – Normalized or Normalized Formed Steel (+N)
- EN 10273 Grade P355NH – Normalized & Normalized-Formed (N) High‑Temperature Steel for Pressure Vessels
- EN 10273 P265GH (Normalized / Normalized‑Formed +N) – Premium High‑Temperature Steel for Boiler & Pressure Vessel Engineering
- EN 10273 Grade P235GH – Normalized/Normalized Formed (+N) High‑Temperature Steel