EN 573-3 Grade AW-1098 O – Food Safe Aluminum with High Strength and Corrosion Resistance
Food safe aluminum.
Properties
General
| Property | Temperature | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|---|
Density | 2.7 g/cm³ | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
20.0 °C | 2.7 g/cm³ | O | EN 573-3 | Rod, Sheet, Strip, Wire |
Mechanical
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Elastic modulus | -270 °C | 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Wire, Rod | |
-270.0 °C | 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Wire, Rod | ||
70.0 GPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |||
20 °C | 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Wire, Rod | ||
20.0 °C | 70.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Wire, Rod | ||
20.0 °C | 70.0 - 72.0 GPa | O | EN 573-3 | Wire, Rod, Sheet, Strip | ||
20.0 °C | 72.0 GPa | O | EN 573-3 | Wire | ||
50.0 °C | 69.0 GPa | O | EN 573-3 | Wire, Rod, Sheet, Strip | ||
100.0 °C | 68.0 GPa | O | EN 573-3 | Wire, Rod, Sheet, Strip | ||
150.0 °C | 66.0 GPa | O | EN 573-3 | Wire, Rod, Sheet, Strip | ||
200.0 °C | 63.0 GPa | O | EN 573-3 | Wire, Rod, Sheet, Strip | ||
250.0 °C | 57.0 GPa | O | EN 573-3 | Wire, Rod, Sheet, Strip | ||
300 °C | 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Wire, Rod | ||
300.0 °C | 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Wire, Rod | ||
Elongation | 25.0 % | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | ||
29.0 % | O | EN 573-3 | Strip, Sheet, Plate | |||
30.0 % | O | EN 573-3 | Strip, Sheet, Plate | |||
33.0 % | O | EN 573-3 | Strip, Sheet, Plate | |||
20.0 °C | 25.0 % | O | EN 573-3 | Wire | A100 | |
20.0 °C | 29.0 % | O | EN 573-3 | Rod | ||
20.0 °C | 30.0 % | O | EN 573-3 | Sheet, Strip | ||
20.0 °C | 33.0 % | O | EN 573-3 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 25.0 - 26.5 GPa | O | EN 573-3 | Rod, Sheet, Strip, Wire | |
Tensile strength | 40.0 MPa | O | EN 573-3 | Strip, Sheet, Plate | ||
70.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |||
20.0 °C | 40.0 MPa | O | EN 573-3 | Rod, Sheet, Strip | ||
20.0 °C | 70.0 MPa | O | EN 573-3 | Wire |
Thermal
| Property | Temperature | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.18e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire |
-50.0 °C | 2.18e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
20 °C | 2.18e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
20 °C | 2.35e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
20 °C | 2.45e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
20 °C | 2.55e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
100 °C | 2.35e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
100.0 °C | 2.36e-05 1/K | O | EN 573-3 | Rod, Sheet, Strip, Wire | |
200 °C | 2.45e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
200.0 °C | 2.45e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
300 °C | 2.55e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
300.0 °C | 2.55e-05 1/K | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Rod, Wire | |
Melting point | 660.0 °C | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
Specific heat capacity | 900.0 J/(kg·K) | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
20.0 °C | 900.0 J/(kg·K) | O | EN 573-3 | Rod, Sheet, Strip, Wire | |
Thermal conductivity | 232 W/(m·K) | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
20.0 °C | 215.0 - 227.0 W/(m·K) | O | EN 573-3 | Rod, Sheet, Strip, Wire |
Electrical
| Property | Temperature | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|---|
Electrical conductivity | 37500000.0 - 37700000.0 S/m | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
20.0 °C | 37600000.0 - 37800000.0 S/m | O | EN 573-3 | Rod, Sheet, Strip, Wire | |
Electrical resistivity | 2.65e-08 - 2.67e-08 Ω·m | O | EN 573-3, EN 1301 | Strip, Sheet, Plate |
Chemical properties
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Aluminium | 99.98 % | O | EN 573-3, EN 1301 | Rod, Sheet, Strip, Wire, Plate |
Copper | 0.003 % | O | EN 573-3, EN 1301 | Rod, Sheet, Strip, Wire, Plate |
Iron | 0.006 % | O | EN 573-3 | Rod, Sheet, Strip, Wire |
0.006 % | O | EN 573-3, EN 1301 | Strip, Sheet, Plate | |
Silicon | 0.01 % | O | EN 573-3, EN 1301 | Rod, Sheet, Strip, Wire, Plate |
Titanium | 0.003 % | O | EN 573-3, EN 1301 | Rod, Sheet, Strip, Wire, Plate |
Zinc | 0.015 % | O | EN 573-3, EN 1301 | Rod, Sheet, Strip, Wire, Plate |
Technological properties
| Property | ||
|---|---|---|
| Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good, general: very good | |
| Corrosion properties | Seawater: acceptable, weathering: good | |
| Workability | Bending / Spinning (cold): very good | |
Metal
- EN 573-3 Grade 3.0505 F Aluminium Alloy: Properties & Standards
- EN 573-3 Grade 3.1305 F Aluminium Alloy – Key Mechanical Properties
- EN 573-3 Grade 3.1305 O Aluminium: Key Mechanical Properties & Standards
- EN 573-3 Grade 3.1305 O3 – Comprehensive Aluminium Alloy Specifications
- EN 573-3 Grade 3.3316 F – Key Properties & Standards for 5000 Series Aluminium
- EN 573-3 Grade 3.3549 F – Premium Aluminum Alloy with Expert R&D Support
- EN 573-3 AW‑1090 F Aluminium: Technical Specifications & Standards
- AW-1098 F Aluminium – EN 573-3 Grade & Core Mechanical Properties
- AW-1098 H14 Aluminum – EN 573-3 Certified Food‑Safe Grade
- EN 573-3 Grade AW-1098 H18 – Food‑Safe Aluminum with Superior Mechanical Properties