Alloy 42 Annealed Strip/Coil – Premium Nickel‑Iron Alloy with Superior Mechanical Properties
A controlled expansion nickel iron alloy, consisting of nearly 41% nickel, balance iron.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 23.0 °C | 8.12 g/cm³ |
Dimension
| Property | Value |
|---|---|
Thickness | 0.25 - 2.03 mm |
Width | 304.8 mm |
Dimensions | Available thicknesses: 0.254mm, 0.381mm, 0.508mm, 2.032mm |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | 23.0 °C | 148 GPa | |
Elongation | 23.0 °C | 30 % | in 2 in. |
Hardness, Rockwell B | 23.0 °C | 80 [-] | |
Tensile strength | 23.0 °C | 566 MPa | |
Yield strength | 23.0 °C | 235 MPa |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 4.2E-6 1/K | from 30°C to the mentioned temperature |
150.0 °C | 4.2E-6 1/K | from 30°C to the mentioned temperature | |
200.0 °C | 4.2E-6 1/K | from 30°C to the mentioned temperature | |
250.0 °C | 4.2E-6 1/K | from 30°C to the mentioned temperature | |
300.0 °C | 4E-6 - 4.7E-6 1/K | from 30°C to the mentioned temperature | |
325.0 °C | 4.6E-6 1/K | from 30°C to the mentioned temperature | |
350.0 °C | 5E-6 1/K | from 30°C to the mentioned temperature | |
375.0 °C | 5.6E-6 1/K | from 30°C to the mentioned temperature | |
400.0 °C | 6.1E-6 1/K | from 30°C to the mentioned temperature | |
425.0 °C | 6.7E-6 1/K | from 30°C to the mentioned temperature | |
450.0 °C | 6.7E-6 - 7.4E-6 1/K | from 30°C to the mentioned temperature | |
475.0 °C | 7.7E-6 1/K | from 30°C to the mentioned temperature | |
500.0 °C | 8.1E-6 1/K | from 30°C to the mentioned temperature | |
525.0 °C | 8.5E-6 1/K | from 30°C to the mentioned temperature | |
550.0 °C | 8.9E-6 1/K | from 30°C to the mentioned temperature | |
600.0 °C | 9.6E-6 1/K | from 30°C to the mentioned temperature | |
700.0 °C | 1.05E-5 1/K | from 30°C to the mentioned temperature | |
800.0 °C | 1.14E-5 1/K | from 30°C to the mentioned temperature | |
900.0 °C | 1.23E-5 1/K | from 30°C to the mentioned temperature | |
1005.0 °C | 1.32E-5 1/K | from 30°C to the mentioned temperature | |
Melting point | 1427 °C | ||
Specific heat capacity | 23.0 °C | 502 J/(kg·K) | |
Thermal conductivity | 23.0 °C | 11 W/(m·K) | |
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 23.0 °C | 6.8E-7 Ω·m |
Magnetic
| Property | Value |
|---|---|
Curie temperature | 380 °C |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.05 % |
Chromium | 0.03 % |
Iron | Balance |
Nickel | 41 % |
Silicon | 0.3 % |
Sulfur | 0.025 % |
Technological properties
| Property | ||
|---|---|---|
| Application areas | Common applications of Alloy 42: Thermostats, thermoswitches, integrated circuit lead frames, Glass to metal seals for a wide variety of electronic tubes, hermetic packages, and automotive and industrial lamps., high temperature curing of aircraft thermoset composites | |
Metal
- Alloy 390E EHT Strip – High-Performance Copper‑Beryllium for Reliable Signal and Power Interconnects
- Alloy 46 (Ni-Fe) Annealed Strip/Coil – High-Strength, Controlled Expansion
- High‑Strength Alloy 25 Strip – Superior Conductivity & Formability
- High-Strength Alloy 25 Strip TH01 (C17200) – Superior Conductivity & Ductility
- Alloy 25 Strip TH02 (C17200): Premium High‑Strength Copper Alloy with Superior Conductivity
- Alloy 25 Strip TH04 (C17200) – High Strength, Superior Conductivity Copper Alloy
- UGIMA® 4571 Annealed – Superior Machinability Stainless Steel
- Alloy 52 Strip/Coil – 51% Ni Controlled Expansion Steel for High‑Performance Applications
- Alloy 42 Annealed Sheet – High‑Strength Nickel‑Iron Alloy for Industrial Use
- Alloy 42 (Nickel‑Iron) Annealed Plate – High Strength & Corrosion Resistance