EN 10297‑1 Grade C55 Quenched & Tempered Steel – Specifications & Mechanical Properties

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.8 - 7.85 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

217 GPa

20.0 °C

210 - 212 GPa

100.0 °C

205 - 207 GPa

200.0 °C

195 - 199 GPa

300.0 °C

185 - 192 GPa

400.0 °C

175 - 184 GPa

500.0 °C

175 GPa

600.0 °C

164 GPa

Elongation

20.0 °C

12 - 15 %

Elongation, transverse

20.0 °C

10 - 13 %

Poisson's ratio

23.0 °C

0.29 [-]

Typical for Medium Carbon Steel

Reduction of area

20.0 °C

30 - 40 %

Reduction of area, transverse

20.0 °C

35 - 45 %

Shear modulus

20.0 °C

81 GPa

Tensile strength

20.0 °C

660 - 1000 MPa

Tensile strength, transverse

20.0 °C

660 - 1000 MPa

Yield strength

20.0 °C

390 - 550 MPa

Yield strength, transverse

20.0 °C

390 - 550 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.08E-5 1/K

20.0 °C

1.19E-5 1/K

100.0 °C

1.11E-5 - 1.25E-5 1/K

200.0 °C

1.21E-5 - 1.3E-5 1/K

300.0 °C

1.29E-5 - 1.36E-5 1/K

400.0 °C

1.35E-5 - 1.41E-5 1/K

500.0 °C

1.45E-5 1/K

600.0 °C

1.49E-5 1/K

Max service temperature

500 °C

Typical for Carbon Steel

Melting point

1380 - 1514 °C

Typical for Medium Carbon Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

20.0 °C

460 - 461 J/(kg·K)

100.0 °C

479 J/(kg·K)

200.0 °C

499 J/(kg·K)

300.0 °C

517 J/(kg·K)

400.0 °C

536 J/(kg·K)

500.0 °C

558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Thermal conductivity

20.0 °C

41.7 - 52 W/(m·K)

100.0 °C

43.4 - 50.6 W/(m·K)

200.0 °C

43.2 - 48.1 W/(m·K)

300.0 °C

41.4 - 45.7 W/(m·K)

400.0 °C

39.1 W/(m·K)

500.0 °C

36.7 W/(m·K)

600.0 °C

34.1 W/(m·K)

Thermal diffusivity

20.0 °C

11.6 mm²/s

100.0 °C

11.3 mm²/s

200.0 °C

10.5 mm²/s

300.0 °C

9.5 mm²/s

400.0 °C

8.3 mm²/s

500.0 °C

7.1 mm²/s

600.0 °C

5.8 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.2E-7 - 2.5E-7 Ω·m

100.0 °C

2.95E-7 Ω·m

200.0 °C

3.65E-7 Ω·m

300.0 °C

4.53E-7 Ω·m

400.0 °C

5.56E-7 Ω·m

500.0 °C

6.74E-7 Ω·m

600.0 °C

8.13E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.52 - 0.6 %

Manganese

0.6 - 0.9 %

Phosphorus

0.05 %

Silicon

0.4 %

Sulfur

0.045 %


Metal

  1. EN 10297-1 Grade 25CrMo4 Quenched & Tempered Steel – Properties & Applications
  2. EN 10297‑1 Grade 30CrMoV9: Quenched & Tempered Steel (QT) – Key Mechanical & Physical Properties
  3. EN 10297‑1 Grade 30CrNiMo8 (QT) – Comprehensive Mechanical & Physical Properties
  4. EN 10297-1 Grade 34CrMo4 Quenched & Tempered Steel – Properties & Performance
  5. EN 10297-1 Grade 34CrNiMo6 – Quenched & Tempered Steel: Detailed Mechanical Properties
  6. EN 10297-1 Grade 41Cr4 Quenched & Tempered Steel – Properties & Performance
  7. EN 10297-1: Grade 36Mn5 Quenched & Tempered Steel – Specifications & Properties
  8. EN 10297-1 Grade Cm60 – Quenched & Tempered Steel: High Strength & Reliability
  9. EN 10297‑1 Grade 28Mn6 Quenched & Tempered Steel (QT) – Key Mechanical Properties
  10. EN 10297-1 Grade 36CrNiMo4 Quenched & Tempered Steel – Key Properties & Applications