Industrial manufacturing
Industrial Internet of Things | Industrial materials | Equipment Maintenance and Repair | Industrial programming |
home  MfgRobots >> Industrial manufacturing >  >> Industrial materials >> Metal

EN 12163 Grade CuSn6 R400: Premium Tin‑Copper Alloy with Superior Corrosion Resistance

CuSn6, mat. No. CW425K, is comparable to the DIN-make CuSn6, mat. No. 2.1020, acc. to DIN 17662 : 1983-12. Properties of the CuSn-alloy are predominantly determined by the tin-content. Tensile strength, yield point and hardness increase according to the rising cold forming grade, elongation after fracture decreases. Electrical and thermal conductivity are lower than for pure copper. Very high resistance to corrosion, particularly to atmospheric influences, seawater, sulfite liquor, carbonated and salted mine water. The alloys are stress corrosion-proof. Processing properties: warm forming: medium cold forming: very good machinability: medium hard soldering: good soft soldering: good gas shielded welding: good burnishing: good Appliction: For all types of springs, especially in electrical industry, for connectors, hose and spring tubes, fabric and screening wires, gong bars. Further application in paper, cellulose and chemical industry, in shipbuilding and machine engineering. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.8 - 8.82 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

118 GPa

Elongation

20.0 °C

26 - 30 %

Elongation A10

20.0 °C

22 %

Elongation A100

20.0 °C

18 %

Poisson's ratio

20.0 °C

0.34 [-]

Tensile strength

20.0 °C

400 MPa

Yield strength Rp0.2

20.0 °C

200 - 250 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

100.0 °C

1.8E-5 1/K

200.0 °C

1.85E-5 1/K

650.0 °C

2.22E-5 1/K

800.0 °C

2.18E-5 1/K

Max service temperature, long

0 - 150 °C

Specific heat capacity

20.0 °C

377 J/(kg·K)

Thermal conductivity

20.0 °C

75 W/(m·K)

200.0 °C

98 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical conductivity

20.0 °C

9.00E+6 S/m

200.0 °C

7.80E+6 S/m

Electrical resistivity

20.0 °C

1.11E-7 Ω·m

200.0 °C

1.28E-7 Ω·m

Specific Electrical conductivity

16 % IACS

Chemical properties

PropertyValue

Iron

0.1 %

Lead

0.02 %

Nickel

0.2 %

Phosphorus

0.01 - 0.4 %

Tin

5.5 - 7 %

Zinc

0.2 %


Metal

  1. EN 12163 Grade CuZn36Sn1Pb R400 – High-Performance Copper‑Brass Alloy
  2. EN 12163 CuZr TH Grade – High Strength Low‑Alloy Copper Alloy
  3. EN 12163 Grade CuSn6 H085: Premium Tin-Copper Alloy for High-Performance Applications
  4. EN 12163 Grade CuSn6 H120 – Premium Tin-Copper Alloy for High-Performance Applications
  5. EN 12163 Grade CuSn6 (H155) – High-Performance Tin-Copper Alloy
  6. EN 12163 CuSn6 R550 – Premium Copper‑Tin Alloy with Superior Corrosion Resistance
  7. EN 12163 Grade CuSn6 R470 – High-Performance Tin‑Copper Alloy
  8. EN 12163 Grade CuNi18Zn20 R400 – Premium High-Strength Copper‑Nickel‑Zinc Alloy
  9. EN 12163 Grade CuZn39Sn1 R400 – Premium Copper Alloy for Industrial Applications
  10. EN 12163 Grade CuSn6 R340 – Premium Tin‑Copper Alloy for Superior Corrosion Resistance