EN 10277-5 Grade Cm45 Cold-Drawn Steel: High Workability & Consistent Mechanical Properties
Steel Cm 45 is suitable for mean strained parts in vehicle manufacturing, engine and machine engineering with enhanced workability and constant mechanical qualities (e.g. transmission shafts, gear wheels, clutch parts, bolts). Lowest application temp. -25 °C.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.8 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Elongation | 20.0 °C | 4 - 8 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Medium Carbon Steel |
Shear modulus | 23.0 °C | 75 - 80 GPa | Typical for Carbon Steel |
Tensile strength | 20.0 °C | 580 - 770 MPa | |
Yield strength | 20.0 °C | 330 - 640 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K | ||
Max service temperature | 500 °C | Typical for Carbon Steel | |
Max service temperature, long | -25 - 0 °C | ||
Melting point | 1380 - 1514 °C | Typical for Medium Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41.7 W/(m·K) | |
100.0 °C | 43.4 W/(m·K) | ||
200.0 °C | 43.2 W/(m·K) | ||
300.0 °C | 41.4 W/(m·K) | ||
400.0 °C | 39.1 W/(m·K) | ||
500.0 °C | 36.7 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.6 mm²/s | |
100.0 °C | 11.3 mm²/s | ||
200.0 °C | 10.5 mm²/s | ||
300.0 °C | 9.5 mm²/s | ||
400.0 °C | 8.3 mm²/s | ||
500.0 °C | 7.1 mm²/s | ||
600.0 °C | 5.8 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.5E-7 Ω·m |
100.0 °C | 2.95E-7 Ω·m | |
200.0 °C | 3.65E-7 Ω·m | |
300.0 °C | 4.53E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m | |
500.0 °C | 6.74E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.42 - 0.5 % |
Manganese | 0.5 - 0.8 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.02 - 0.035 % |
Metal
- EN 10277-5 Grade 25CrMo4 Cold-Drawn Steel – High Strength & Ductility
- EN 10277-5 Grade 25CrMoS4 Cold-Drawn Steel – High Strength & Ductility for Automotive & Industrial Applications
- EN 10277-5 Grade 38Cr2 Cold Drawn Steel – High Strength & Low-Temperature Performance
- EN 10277-5 Grade 38CrS2 Cold Drawn Steel – Precision Alloy for Automotive and Machinery
- EN 10277‑5 Grade 41Cr4 Cold‑Drawn Steel – High‑Performance for Automotive & Machine Engineering
- EN 10277-5 Grade 41CrS4 Cold-Drawn Steel – High Strength for Automotive and Industrial Applications
- EN 10277-5 Grade 42CrMo4 – Premium Cold‑Drawn Steel for Heavy‑Duty Applications
- EN 10277‑5 Grade 46Cr2 Cold‑Drawn Steel – High Strength, Low Ductility for Vehicle Components
- EN 10277-5 Grade 46CrS2 Cold Drawn Steel – High Strength & Workability
- EN 10277-5 Grade 50CrMo4 Cold Drawn Steel – High‑Strength, Low‑Temperature Performance