EN 10250-4 X3CrNiMo17-13-3 Solution-Annealed Steel: Superior Corrosion Resistance for Chemical Applications
The make X3CrNiMo17-13-3 is comparable to X5 CrNiMo 17 13 3 acc. to DIN17440 : 1985-07. Corrosion behaviour is similar to 1.4401. Slightly improved resistance to selective attack due to the higher Mo-content. In delivery condition resistant to intercrystalline corrosion. Application in chemical and pharmaceutical industry for acid resistant instruments, in cellulose, coloring, fatty acid, textile and rayon industry as well as in petrochemical industry.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 8 - 8.01 g/cm³ |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | -100.0 °C | 206 GPa |
20.0 °C | 196 - 200 GPa | |
100.0 °C | 190 - 194 GPa | |
200.0 °C | 182 - 186 GPa | |
300.0 °C | 174 - 179 GPa | |
400.0 °C | 166 - 172 GPa | |
500.0 °C | 158 - 165 GPa | |
600.0 °C | 150 GPa | |
700.0 °C | 142 GPa | |
800.0 °C | 134 GPa | |
Elongation, transverse | 20.0 °C | 30 % |
Poisson's ratio | 20.0 °C | 0.28 [-] |
Shear modulus | 20.0 °C | 77.3 GPa |
Tensile strength, transverse | 20.0 °C | 500 - 700 MPa |
Yield strength Rp0.2 | 100.0 °C | 177 MPa |
150.0 °C | 162 MPa | |
200.0 °C | 147 MPa | |
250.0 °C | 137 MPa | |
300.0 °C | 127 MPa | |
350.0 °C | 120 MPa | |
400.0 °C | 115 MPa | |
450.0 °C | 112 MPa | |
500.0 °C | 110 MPa | |
550.0 °C | 108 MPa | |
Yield strength Rp0.2, transverse | 20.0 °C | 200 MPa |
Yield strength Rp1.0 | 100.0 °C | 211 MPa |
150.0 °C | 191 MPa | |
200.0 °C | 177 MPa | |
250.0 °C | 167 MPa | |
300.0 °C | 156 MPa | |
350.0 °C | 150 MPa | |
400.0 °C | 144 MPa | |
450.0 °C | 141 MPa | |
500.0 °C | 139 MPa | |
550.0 °C | 137 MPa | |
Yield strength Rp1.0, transverse | 20.0 °C | 235 MPa |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K | ||
Melting point | 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 13.5 - 15 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) | ||
200.0 °C | 16.7 W/(m·K) | ||
300.0 °C | 18.3 W/(m·K) | ||
400.0 °C | 19.8 W/(m·K) | ||
500.0 °C | 21.3 W/(m·K) | ||
600.0 °C | 22.7 W/(m·K) | ||
700.0 °C | 24.2 W/(m·K) | ||
800.0 °C | 25.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.6 mm²/s | |
100.0 °C | 3.7 mm²/s | ||
200.0 °C | 4 mm²/s | ||
300.0 °C | 4.4 mm²/s | ||
400.0 °C | 4.6 mm²/s | ||
500.0 °C | 4.7 mm²/s | ||
600.0 °C | 4.9 mm²/s | ||
700.0 °C | 5.2 mm²/s | ||
800.0 °C | 5.5 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 7.75E-7 Ω·m |
100.0 °C | 8.42E-7 Ω·m | |
200.0 °C | 9.04E-7 Ω·m | |
300.0 °C | 9.62E-7 Ω·m | |
400.0 °C | 1.01E-6 Ω·m | |
500.0 °C | 1.06E-6 Ω·m | |
600.0 °C | 1.1E-6 Ω·m | |
700.0 °C | 1.13E-6 Ω·m | |
800.0 °C | 1.16E-6 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.05 % |
Chromium | 16.5 - 18.5 % |
Manganese | 2 % |
Molybdenum | 2.5 - 3 % |
Nickel | 10.5 - 13 % |
Nitrogen | 0.11 % |
Phosphorus | 0.05 % |
Silicon | 1 % |
Sulfur | 0.03 % |
Metal
- EN 10250-4 Grade X2CrNiMoCuN25-6-3 – Solution Annealed Steel for High-Performance Applications
- EN 10250-4 Grade X2CrNiMoCuWN25-7-4 – Solution Annealed for High-Performance Applications
- EN 10250-4 Grade X2CrNiMoN25-7-4: Solution-Annealed Steel for High-Performance Applications
- EN 10250-4 Grade X1CrNiMoCuN20-18-7 – Solution Annealed Stainless Steel for High-Performance Applications
- EN 10250-4 X2CrNi18-9 Austenitic Steel – Solution Annealed + AT
- EN 10250-4 X2CrNiN23-4 Duplex Stainless Steel – Solution Annealed (+AT)
- EN 10250-4 Grade X3CrNiMoN27-5-2 Solution Annealed – High-Performance Stainless Steel for Corrosion Resistance
- EN 10250-4 X2CrNi19-11 Stainless Steel – Solution Annealed (+AT) – High Corrosion Resistance & Premium Quality
- EN 10250-4 Grade X2CrNiMo17-12-2 Solution-Annealed Steel (+AT) – High Corrosion Resistance
- EN 10250-4 X2CrNiMoN17-11-2 Solution-Annealed Steel for High-Performance Chemical Applications