DIN 17179 Grade WStE 460 – Normalized/Normalized Formed Steel Tubes (+N)
The fine grained steel is used acc. DIN 17178 : 1986-5 for welded steel tubes and acc. DIN 17179 : 1986-5 as seamless steel tubes for special purposes from -20 to 400 degrees C. Application: pressure vessel construction, apparatus construction, pipelines, mechanical engineering, toolbuilding Special requirements regarding processing have to be arranged (e.g. coatings). For welded tubes the calculation with the 100 % loads are possible for the seam area.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.84 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Elongation | 20.0 °C | 19 % | |
Elongation, transverse | 20.0 °C | 17 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] | Typical for Steel |
Tensile strength | 20.0 °C | 490 - 730 MPa | |
100.0 °C | 470 - 510 MPa | ||
150.0 °C | 450 - 490 MPa | ||
200.0 °C | 440 - 480 MPa | ||
250.0 °C | 440 - 480 MPa | ||
300.0 °C | 440 - 480 MPa | ||
350.0 °C | 430 - 470 MPa | ||
400.0 °C | 420 - 460 MPa | ||
Tensile strength, transverse | 20.0 °C | 490 - 730 MPa | |
Yield strength | 20.0 °C | 390 - 460 MPa | |
Yield strength Rp0.2 | 100.0 °C | 353 - 402 MPa | |
150.0 °C | 324 - 373 MPa | ||
200.0 °C | 304 - 343 MPa | ||
250.0 °C | 275 - 314 MPa | ||
300.0 °C | 255 - 294 MPa | ||
350.0 °C | 226 - 265 MPa | ||
400.0 °C | 196 - 235 MPa | ||
Yield strength, transverse | 20.0 °C | 390 - 460 MPa | |
Thermal
| Property | Temperature | Value |
|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 - 1.08E-5 1/K |
20.0 °C | 1.15E-5 - 1.19E-5 1/K | |
100.0 °C | 1.21E-5 - 1.25E-5 1/K | |
200.0 °C | 1.27E-5 - 1.3E-5 1/K | |
300.0 °C | 1.32E-5 - 1.36E-5 1/K | |
400.0 °C | 1.36E-5 - 1.41E-5 1/K | |
500.0 °C | 1.4E-5 - 1.45E-5 1/K | |
600.0 °C | 1.44E-5 - 1.49E-5 1/K | |
Max service temperature, long | -20 - 400 °C | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) | |
Thermal conductivity | -100.0 °C | 34.7 W/(m·K) |
20.0 °C | 39.7 W/(m·K) | |
100.0 °C | 40.9 W/(m·K) | |
200.0 °C | 41 W/(m·K) | |
300.0 °C | 39.9 W/(m·K) | |
400.0 °C | 38.2 W/(m·K) | |
500.0 °C | 36.1 W/(m·K) | |
600.0 °C | 33.8 W/(m·K) | |
Thermal diffusivity | -100.0 °C | 11.9 mm²/s |
20.0 °C | 11 mm²/s | |
100.0 °C | 10.5 mm²/s | |
200.0 °C | 9.9 mm²/s | |
300.0 °C | 9.1 mm²/s | |
400.0 °C | 8.1 mm²/s | |
500.0 °C | 6.9 mm²/s | |
600.0 °C | 5.7 mm²/s | |
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | -100.0 °C | 1.97E-7 Ω·m |
20.0 °C | 2.62E-7 Ω·m | |
100.0 °C | 3.13E-7 Ω·m | |
200.0 °C | 3.85E-7 Ω·m | |
300.0 °C | 4.7E-7 Ω·m | |
400.0 °C | 5.69E-7 Ω·m | |
500.0 °C | 6.85E-7 Ω·m | |
600.0 °C | 8.2E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Aluminium | 0.02 % |
Carbon | 0.2 % |
Chromium | 0.3 % |
Copper | 0.2 % |
Manganese | 1 - 1.7 % |
Molybdenum | 0.1 % |
Nickel | 1 % |
Nitrogen | 0.02 % |
Phosphorus | 0.04 % |
Silicon | 0.1 - 0.6 % |
Sulfur | 0.03 % |
Titanium | 0.2 % |
Vanadium | 0.22 % |
Metal
- DIN 17103 WStE 460 Steel: Normalized & Normalized Formed (+N) for High-Temperature Applications
- DIN 17125 Grade EStE 460 – Premium Normalized Steel Tubes (+N)
- DIN 17125 Grade TStE 460 – Normalized or Normalized‑Formed Steel for High‑Temperature Applications
- DIN 17179 WStE 420 Steel Tubes – Normalized/Normalized Formed Grade for High-Performance Applications
- WStE 285 Steel (DIN 17103) – Normalized or Normalized Formed (N): Properties & Applications
- DIN 17103 WStE 355: High-Temperature Grade Steel – Normalized or Normalized +N
- DIN 17125 Grade StE 460 – Normalized or Normalized Formed Steel
- DIN 17179 Grade WStE 255: Normalized or Normalized‑Formed Steel Tubes for High‑Temperature Applications
- DIN 17179 Grade WStE 285 – Normalized and Normalized‑Formed Steel Tubes
- DIN 17179 Grade WStE 355 – Normalized & Normalized-Formed Steel Tubes