EN 10277-2 Grade St 44-3: Fine-Grained Cold-Drawn or Turned and Normalized Steel

St 44-3 is a fine grained steel for welded constructions up to a temperature of -20 °C.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.85 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

217 GPa

20.0 °C

212 GPa

100.0 °C

207 GPa

200.0 °C

199 GPa

300.0 °C

192 GPa

400.0 °C

184 GPa

500.0 °C

175 GPa

600.0 °C

164 GPa

Elongation

20.0 °C

20 - 22 %

Poisson's ratio

20.0 °C

0.28 [-]

Shear modulus

23.0 °C

82 GPa

Typical for Low Carbon Steel

Tensile strength

20.0 °C

410 - 560 MPa

Yield strength

20.0 °C

245 - 275 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.08E-5 1/K

20.0 °C

1.19E-5 1/K

100.0 °C

1.25E-5 1/K

200.0 °C

1.3E-5 1/K

300.0 °C

1.36E-5 1/K

400.0 °C

1.41E-5 1/K

500.0 °C

1.45E-5 1/K

600.0 °C

1.49E-5 1/K

Max service temperature

500 °C

Typical for Carbon Steel

Max service temperature, long

-20 - 0 °C

Melting point

1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

20.0 °C

461 J/(kg·K)

100.0 °C

479 J/(kg·K)

200.0 °C

499 J/(kg·K)

300.0 °C

517 J/(kg·K)

400.0 °C

536 J/(kg·K)

500.0 °C

558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Thermal conductivity

20.0 °C

53.4 W/(m·K)

100.0 °C

52.9 W/(m·K)

200.0 °C

50.3 W/(m·K)

300.0 °C

46.7 W/(m·K)

400.0 °C

43.3 W/(m·K)

500.0 °C

39.8 W/(m·K)

600.0 °C

36.7 W/(m·K)

Thermal diffusivity

20.0 °C

14.8 mm²/s

100.0 °C

13.6 mm²/s

200.0 °C

12.1 mm²/s

300.0 °C

10.6 mm²/s

400.0 °C

9.2 mm²/s

500.0 °C

7.7 mm²/s

600.0 °C

6.2 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.95E-7 Ω·m

100.0 °C

2.42E-7 Ω·m

200.0 °C

3.14E-7 Ω·m

300.0 °C

4.02E-7 Ω·m

400.0 °C

5.02E-7 Ω·m

500.0 °C

6.21E-7 Ω·m

600.0 °C

7.55E-7 Ω·m

Magnetic

PropertyValueComment

Curie temperature

770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValue

Aluminium

0.02 %

Carbon

0.2 %

Phosphorus

0.04 %

Sulfur

0.04 %


Metal

  1. EN 10277‑2 Grade ZSt50‑2: Cold‑Drawn & Turned High‑Strength Steel
  2. EN 10277-2 Grade ZSt60-2: Cold‑Drawn, Turned & Normalized Steel for High‑Strength Applications
  3. EN 10277-2 Grade ZSt70-2: High-Performance Cold-Drawn & Normalized Steel for Wear-Resistant Applications
  4. EN 10277-2 Grade St 50-2: Premium Cold‑Drawn Structural Steel for High‑Performance Applications
  5. EN 10277-2 Grade St 60-2 – Premium Cold‑Drawn, Turned, and Normalized Structural Steel
  6. EN 10277-2 Grade St 70-2 – Cold Drawn or Turned, Normalized Structural Steel
  7. EN 10277-2 Grade St 37-2: Cold Drawn, Turned & Normalized Low‑Carbon Steel
  8. EN 10277-2 Grade ZSt52-3: Cold-Drawn, Turned, and Normalized High-Strength Structural Steel
  9. EN 10277-2: Grade St52-3 – Cold Drawn or Turned and Normalized Steel for High-Dynamic Load Applications
  10. EN 10277‑2 Grade ZSt 44‑3: Cold‑Drawn, Turned & Normalized Steel for Dynamic Welded Structures