EN 10263-4 Grade 46Cr2 Steel – Cold Drawn, Annealed for Spheroidized Carbides with Light Skin Pass
Because of its high carbon content, the cold-upsettable steel 46 Cr 2 can be processed in cold condition only with a small to medium rate of forming. It is used for screws and bolts of strength class 8.8 in the lower dimension range. The steel 46 Cr 2 will be replaced with steel 35 B 2.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.8 g/cm³ |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa |
20.0 °C | 212 GPa | |
100.0 °C | 207 GPa | |
200.0 °C | 199 GPa | |
300.0 °C | 192 GPa | |
400.0 °C | 184 GPa | |
500.0 °C | 175 GPa | |
600.0 °C | 164 GPa | |
Poisson's ratio | 20.0 °C | 0.28 [-] |
Reduction of area | 20.0 °C | 60 % |
Tensile strength | 20.0 °C | 600 - 620 MPa |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K | ||
Melting point | 1382 - 1529 °C | Typical for Chromium Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 44.9 W/(m·K) | |
100.0 °C | 46.2 W/(m·K) | ||
200.0 °C | 45.5 W/(m·K) | ||
300.0 °C | 43.1 W/(m·K) | ||
400.0 °C | 40.4 W/(m·K) | ||
500.0 °C | 37.7 W/(m·K) | ||
600.0 °C | 34.9 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 12.5 mm²/s | |
100.0 °C | 12 mm²/s | ||
200.0 °C | 11 mm²/s | ||
300.0 °C | 9.8 mm²/s | ||
400.0 °C | 8.6 mm²/s | ||
500.0 °C | 7.3 mm²/s | ||
600.0 °C | 5.9 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.32E-7 Ω·m |
100.0 °C | 2.77E-7 Ω·m | |
200.0 °C | 3.47E-7 Ω·m | |
300.0 °C | 4.35E-7 Ω·m | |
400.0 °C | 5.38E-7 Ω·m | |
500.0 °C | 6.56E-7 Ω·m | |
600.0 °C | 7.95E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.42 - 0.5 % |
Chromium | 0.4 - 0.6 % |
Manganese | 0.5 - 0.8 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.035 % |
Metal
- EN 10263‑4 Grade 38Cr2 Steel: Cold‑Drawn, Annealed, Spheroidized Carbides & Slight Skin Pass
- EN 10263-4 Grade 41Cr4 Steel: Cold‑Drawn, Annealed for Spheroidized Carbides & Enhanced Surface Quality
- EN 10263-4 Grade 42CrMo4: Cold-Drawn, Annealed Steel with Spheroidized Carbides
- EN 10263-4 Grade Cq35 Steel – Cold Drawn, Annealed, Spheroidized Carbides, Skin-Passed
- EN 10263-4 Grade Cq45: Cold‑Drawn, Annealed Steel with Spheroidized Carbides – Ideal for High‑Strength Screws & Nuts
- EN 10263-4 Grade 30CrNiMo8 – Cold-Drawn, Annealed Steel with Spheroidized Carbides & Skin Pass
- EN 10263-4 Grade 34Cr4 Cold-Drawn & Annealed Steel with Spheroidized Carbides – Skin-Passed Finish
- EN 10263‑4 Grade 34CrNiMo6 – Cold‑Drawn, Annealed Steel with Spheroidized Carbides for High‑Strength Applications
- EN 10263-4 Grade 37Cr4 Steel: Cold-Drawn, Annealed with Spheroidized Carbides and Light Skin Pass
- EN 10263-4 Grade 25CrMo4: Cold-Drawn, Annealed Steel with Spheroidized Carbides and Skin Pass