EN 10263-4 Grade 25CrMo4: Cold-Drawn, Annealed Steel with Spheroidized Carbides and Skin Pass
The cold-upsettable steel 25 CrMo 4 can be cold-formed with a medium to high rate of forming according to the usual forming methods on single-stage and multi-stage presses. It is used for screws and pressed parts of strength class in the medium dimension range.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.83 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Poisson's ratio | 20.0 °C | 0.29 [-] | Typical for Chromium Molybdenum Steel |
Reduction of area | 20.0 °C | 62 % | |
Tensile strength | 20.0 °C | 560 - 580 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Max service temperature, long | 0 - 200 °C | ||
Melting point | 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41 W/(m·K) | |
100.0 °C | 42.7 W/(m·K) | ||
200.0 °C | 42.8 W/(m·K) | ||
300.0 °C | 41.6 W/(m·K) | ||
400.0 °C | 39.9 W/(m·K) | ||
500.0 °C | 37.8 W/(m·K) | ||
600.0 °C | 35.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.4 mm²/s | |
100.0 °C | 11 mm²/s | ||
200.0 °C | 10.3 mm²/s | ||
300.0 °C | 9.5 mm²/s | ||
400.0 °C | 8.5 mm²/s | ||
500.0 °C | 7.3 mm²/s | ||
600.0 °C | 6 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.54E-7 Ω·m |
100.0 °C | 3E-7 Ω·m | |
200.0 °C | 3.69E-7 Ω·m | |
300.0 °C | 4.51E-7 Ω·m | |
400.0 °C | 5.45E-7 Ω·m | |
500.0 °C | 6.54E-7 Ω·m | |
600.0 °C | 7.78E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.22 - 0.29 % |
Chromium | 0.9 - 1.2 % |
Manganese | 0.6 - 0.9 % |
Molybdenum | 0.15 - 0.3 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.035 % |
Metal
- EN 10263‑4 Grade 38Cr2 Steel: Cold‑Drawn, Annealed, Spheroidized Carbides & Slight Skin Pass
- EN 10263-4 Grade 41Cr4 Steel: Cold‑Drawn, Annealed for Spheroidized Carbides & Enhanced Surface Quality
- EN 10263-4 Grade 42CrMo4: Cold-Drawn, Annealed Steel with Spheroidized Carbides
- EN 10263-4 Grade 46Cr2 Steel – Cold Drawn, Annealed for Spheroidized Carbides with Light Skin Pass
- EN 10263-4 Grade Cq35 Steel – Cold Drawn, Annealed, Spheroidized Carbides, Skin-Passed
- EN 10263-4 Grade Cq45: Cold‑Drawn, Annealed Steel with Spheroidized Carbides – Ideal for High‑Strength Screws & Nuts
- EN 10263-4 Grade 30CrNiMo8 – Cold-Drawn, Annealed Steel with Spheroidized Carbides & Skin Pass
- EN 10263-4 Grade 34Cr4 Cold-Drawn & Annealed Steel with Spheroidized Carbides – Skin-Passed Finish
- EN 10263‑4 Grade 34CrNiMo6 – Cold‑Drawn, Annealed Steel with Spheroidized Carbides for High‑Strength Applications
- EN 10263-4 Grade 37Cr4 Steel: Cold-Drawn, Annealed with Spheroidized Carbides and Light Skin Pass