Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.85 g/cm³

50.0 °C

7.84 g/cm³

100.0 °C

7.82 g/cm³

150.0 °C

7.81 g/cm³

200.0 °C

7.79 g/cm³

250.0 °C

7.77 g/cm³

300.0 °C

7.76 g/cm³

350.0 °C

7.74 g/cm³

400.0 °C

7.72 g/cm³

450.0 °C

7.7 g/cm³

500.0 °C

7.68 g/cm³

550.0 °C

7.66 g/cm³

600.0 °C

7.64 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

217 GPa

20.0 °C

212 - 212.48 GPa

50.0 °C

211.6 GPa

100.0 °C

207 - 208.95 GPa

150.0 °C

205.52 GPa

200.0 °C

199 - 201.79 GPa

250.0 °C

197.67 GPa

300.0 °C

192 - 193.45 GPa

350.0 °C

189.23 GPa

400.0 °C

184 - 184.82 GPa

450.0 °C

180.41 GPa

500.0 °C

175 - 175.89 GPa

550.0 °C

171.28 GPa

600.0 °C

164 - 166.57 GPa

Poisson's ratio

20.0 °C

0.28 [-]

50.0 °C

0.28 [-]

100.0 °C

0.28 [-]

150.0 °C

0.29 [-]

200.0 °C

0.29 [-]

250.0 °C

0.29 [-]

300.0 °C

0.29 [-]

350.0 °C

0.3 [-]

400.0 °C

0.3 [-]

450.0 °C

0.3 [-]

500.0 °C

0.3 [-]

550.0 °C

0.31 [-]

600.0 °C

0.31 [-]

Shear modulus

20.0 °C

82.8 GPa

50.0 °C

82.4 GPa

100.0 °C

81.42 GPa

150.0 °C

79.95 GPa

200.0 °C

78.38 GPa

250.0 °C

76.62 GPa

300.0 °C

74.85 GPa

350.0 °C

73.08 GPa

400.0 °C

71.32 GPa

450.0 °C

69.45 GPa

500.0 °C

67.59 GPa

550.0 °C

65.63 GPa

600.0 °C

63.57 GPa

Yield strength Rp0.2

50.0 °C

265 MPa

100.0 °C

256 MPa

150.0 °C

242 MPa

200.0 °C

220 - 230 MPa

250.0 °C

210 - 220 MPa

300.0 °C

195 - 205 MPa

350.0 °C

180 - 190 MPa

400.0 °C

168 - 180 MPa

450.0 °C

157 - 170 MPa

500.0 °C

148 - 165 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.05E-5 1/K

20.0 °C

1.15E-5 1/K

100.0 °C

1.21E-5 1/K

200.0 °C

1.27E-5 1/K

300.0 °C

1.32E-5 1/K

400.0 °C

1.36E-5 1/K

500.0 °C

1.4E-5 1/K

600.0 °C

1.44E-5 1/K

Max service temperature, long

400 - 550 °C

Melting point

1382 - 1529 °C

Typical for Chromium Molybdenum Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

20.0 °C

461 J/(kg·K)

100.0 °C

479 J/(kg·K)

200.0 °C

499 J/(kg·K)

300.0 °C

517 J/(kg·K)

400.0 °C

536 J/(kg·K)

500.0 °C

558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Thermal conductivity

20.0 °C

45.9 W/(m·K)

100.0 °C

46.4 W/(m·K)

200.0 °C

45.6 W/(m·K)

300.0 °C

43.5 W/(m·K)

400.0 °C

40.9 W/(m·K)

500.0 °C

38.2 W/(m·K)

600.0 °C

35.5 W/(m·K)

Thermal diffusivity

20.0 °C

12.7 mm²/s

100.0 °C

12 mm²/s

200.0 °C

11 mm²/s

300.0 °C

9.9 mm²/s

400.0 °C

8.7 mm²/s

500.0 °C

7.3 mm²/s

600.0 °C

6 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

2.27E-7 - 2.37E-7 Ω·m

50.0 °C

2.56E-7 Ω·m

100.0 °C

2.76E-7 - 2.88E-7 Ω·m

150.0 °C

3.21E-7 Ω·m

200.0 °C

3.46E-7 - 3.59E-7 Ω·m

250.0 °C

4.01E-7 Ω·m

300.0 °C

4.31E-7 - 4.45E-7 Ω·m

350.0 °C

4.95E-7 Ω·m

400.0 °C

5.32E-7 - 5.48E-7 Ω·m

450.0 °C

6.06E-7 Ω·m

500.0 °C

6.48E-7 - 6.63E-7 Ω·m

550.0 °C

7.28E-7 Ω·m

600.0 °C

7.81E-7 - 7.97E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.08 - 0.18 %

Chromium

0.7 - 1.15 %

Copper

0.3 %

Manganese

0.4 - 1 %

Molybdenum

0.4 - 0.6 %

Nitrogen

0.01 %

Phosphorus

0.03 %

Silicon

0.35 %

Sulfur

0.01 - 0.025 %


Metal

  1. EN 10137-2 Grade S890QL – High-Strength Quenched & Tempered Steel for Heavy-Duty Applications
  2. EN 10137-3 Grade S500A: Quenched & Tempered Fine‑Grained Steel for Structural Applications
  3. EN 10083-1 Grade 51CrV4: Quenched & Tempered Steel (QT)
  4. EN 10213 Grade G17CrMo9-10 – Quenched & Tempered (QT) Steel for High-Temperature Applications
  5. EN 10085 Grade 15 CrMoV 5.9: Quenched & Tempered Steel for Durable Machine Components
  6. EN 10085 Grade 31CrMo12 – High-Performance Quenched & Tempered Steel for Heavy‑Duty Applications
  7. EN 10216-2 Grade 11CrMo9-10 Quenched & Tempered Seamless Tubes – High‑Temperature, High‑Pressure Applications
  8. EN 10132-3: 42CrMo4 Quenched & Tempered Alloy Steel – Premium Cold-Rolled Strips
  9. EN 10273 13CrMo4-5 Steel Bars – Normalized & Tempered or Quenched & Tempered for High-Pressure Applications
  10. EN 10222-2 Grade 13CrMo4-5 – High-Strength Quenched & Tempered Steel for Pressure Vessels