EN 10222-2 Grade 13CrMo4-5 – High-Strength Quenched & Tempered Steel for Pressure Vessels
Material 13CrMo4-5, material number 1.7335 is used in pressure vessel construction. Application in boiler construction, for collectors, flanges and welded collars, in apparatus engineering and in petrochemistry.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.85 g/cm³ |
50.0 °C | 7.84 g/cm³ | |
100.0 °C | 7.82 g/cm³ | |
150.0 °C | 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ | |
250.0 °C | 7.77 g/cm³ | |
300.0 °C | 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ | |
450.0 °C | 7.7 g/cm³ | |
500.0 °C | 7.68 g/cm³ | |
550.0 °C | 7.66 g/cm³ | |
600.0 °C | 7.64 g/cm³ | |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa |
20.0 °C | 212 - 212.48 GPa | |
50.0 °C | 211.6 GPa | |
100.0 °C | 207 - 208.95 GPa | |
150.0 °C | 205.52 GPa | |
200.0 °C | 199 - 201.79 GPa | |
250.0 °C | 197.67 GPa | |
300.0 °C | 192 - 193.45 GPa | |
350.0 °C | 189.23 GPa | |
400.0 °C | 184 - 184.82 GPa | |
450.0 °C | 180.41 GPa | |
500.0 °C | 175 - 175.89 GPa | |
550.0 °C | 171.28 GPa | |
600.0 °C | 164 - 166.57 GPa | |
Elongation | 20.0 °C | 18 - 20 % |
Poisson's ratio | 20.0 °C | 0.28 [-] |
50.0 °C | 0.28 [-] | |
100.0 °C | 0.28 [-] | |
150.0 °C | 0.29 [-] | |
200.0 °C | 0.29 [-] | |
250.0 °C | 0.29 [-] | |
300.0 °C | 0.29 [-] | |
350.0 °C | 0.3 [-] | |
400.0 °C | 0.3 [-] | |
450.0 °C | 0.3 [-] | |
500.0 °C | 0.3 [-] | |
550.0 °C | 0.31 [-] | |
600.0 °C | 0.31 [-] | |
Shear modulus | 20.0 °C | 82.8 GPa |
50.0 °C | 82.4 GPa | |
100.0 °C | 81.42 GPa | |
150.0 °C | 79.95 GPa | |
200.0 °C | 78.38 GPa | |
250.0 °C | 76.62 GPa | |
300.0 °C | 74.85 GPa | |
350.0 °C | 73.08 GPa | |
400.0 °C | 71.32 GPa | |
450.0 °C | 69.45 GPa | |
500.0 °C | 67.59 GPa | |
550.0 °C | 65.63 GPa | |
600.0 °C | 63.57 GPa | |
Tensile strength | 20.0 °C | 420 - 590 MPa |
Yield strength | 20.0 °C | 240 - 275 MPa |
Yield strength Rp0.2 | 20.0 °C | 230 - 265 MPa |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Max service temperature, long | 400 - 550 °C | ||
Melting point | 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 45.9 W/(m·K) | |
100.0 °C | 46.4 W/(m·K) | ||
200.0 °C | 45.6 W/(m·K) | ||
300.0 °C | 43.5 W/(m·K) | ||
400.0 °C | 40.9 W/(m·K) | ||
500.0 °C | 38.2 W/(m·K) | ||
600.0 °C | 35.5 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 12.7 mm²/s | |
100.0 °C | 12 mm²/s | ||
200.0 °C | 11 mm²/s | ||
300.0 °C | 9.9 mm²/s | ||
400.0 °C | 8.7 mm²/s | ||
500.0 °C | 7.3 mm²/s | ||
600.0 °C | 6 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.27E-7 - 2.37E-7 Ω·m |
50.0 °C | 2.56E-7 Ω·m | |
100.0 °C | 2.76E-7 - 2.88E-7 Ω·m | |
150.0 °C | 3.21E-7 Ω·m | |
200.0 °C | 3.46E-7 - 3.59E-7 Ω·m | |
250.0 °C | 4.01E-7 Ω·m | |
300.0 °C | 4.31E-7 - 4.45E-7 Ω·m | |
350.0 °C | 4.95E-7 Ω·m | |
400.0 °C | 5.32E-7 - 5.48E-7 Ω·m | |
450.0 °C | 6.06E-7 Ω·m | |
500.0 °C | 6.48E-7 - 6.63E-7 Ω·m | |
550.0 °C | 7.28E-7 Ω·m | |
600.0 °C | 7.81E-7 - 7.97E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.08 - 0.18 % |
Chromium | 0.7 - 1.15 % |
Copper | 0.3 % |
Manganese | 0.4 - 1 % |
Molybdenum | 0.4 - 0.6 % |
Nickel | 0.3 % |
Phosphorus | 0.03 % |
Silicon | 0.35 % |
Sulfur | 0.01 - 0.015 % |
Metal
- EN 10137-2 Grade S890QL – High-Strength Quenched & Tempered Steel for Heavy-Duty Applications
- EN 10137-3 Grade S500A: Quenched & Tempered Fine‑Grained Steel for Structural Applications
- EN 10083-1 Grade 51CrV4: Quenched & Tempered Steel (QT)
- EN 10213 Grade G17CrMo9-10 – Quenched & Tempered (QT) Steel for High-Temperature Applications
- EN 10085 Grade 15 CrMoV 5.9: Quenched & Tempered Steel for Durable Machine Components
- EN 10085 Grade 31CrMo12 – High-Performance Quenched & Tempered Steel for Heavy‑Duty Applications
- EN 10273 13CrMo4-5 Quenched & Tempered Steel – High-Temperature Performance
- EN 10222-2 Grade 16Mo3 Quenched & Tempered Steel (+QT) – High-Temperature, Pressure Vessel Grade
- EN 10222-2 Grade X20CrMoV11-1 – High‑Temperature Quenched & Tempered Steel (+QT)
- EN 10222-2 Grade P305GH: High‑Temperature Quenched & Tempered Steel for Pressure Vessels