EN 10222-2 Grade 14MoV6-3 – Normalized & Tempered (NT) High-Temperature Steel for Pressure Vessels
The high temperature material 14MoV6-3, material number 1.7715, is used in pressure vessel construction. It is owing to its good high-temperature strength properties favorable at high pressures in a temperature range from 500 to 560 °C. Application for welded collars and flanges.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.84 g/cm³ |
50.0 °C | 7.84 g/cm³ | |
100.0 °C | 7.82 g/cm³ | |
150.0 °C | 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ | |
250.0 °C | 7.78 g/cm³ | |
300.0 °C | 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ | |
450.0 °C | 7.71 g/cm³ | |
500.0 °C | 7.69 g/cm³ | |
550.0 °C | 7.67 g/cm³ | |
600.0 °C | 7.65 g/cm³ | |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa |
20.0 °C | 212 - 212.78 GPa | |
50.0 °C | 211.5 GPa | |
100.0 °C | 207 - 208.66 GPa | |
150.0 °C | 205.23 GPa | |
200.0 °C | 199 - 201.6 GPa | |
250.0 °C | 197.77 GPa | |
300.0 °C | 192 - 193.94 GPa | |
350.0 °C | 189.92 GPa | |
400.0 °C | 184 - 186.1 GPa | |
450.0 °C | 181.98 GPa | |
500.0 °C | 175 - 177.86 GPa | |
550.0 °C | 173.74 GPa | |
600.0 °C | 164 - 169.42 GPa | |
Elongation | 20.0 °C | 18 - 20 % |
Poisson's ratio | 20.0 °C | 0.29 [-] |
50.0 °C | 0.29 [-] | |
100.0 °C | 0.28 [-] | |
150.0 °C | 0.29 [-] | |
200.0 °C | 0.29 [-] | |
250.0 °C | 0.29 [-] | |
300.0 °C | 0.3 [-] | |
350.0 °C | 0.3 [-] | |
400.0 °C | 0.3 [-] | |
450.0 °C | 0.31 [-] | |
500.0 °C | 0.31 [-] | |
550.0 °C | 0.32 [-] | |
600.0 °C | 0.32 [-] | |
Shear modulus | 20.0 °C | 82.8 GPa |
50.0 °C | 82.31 GPa | |
100.0 °C | 81.23 GPa | |
150.0 °C | 79.76 GPa | |
200.0 °C | 78.28 GPa | |
250.0 °C | 76.62 GPa | |
300.0 °C | 74.85 GPa | |
350.0 °C | 73.18 GPa | |
400.0 °C | 71.42 GPa | |
450.0 °C | 69.65 GPa | |
500.0 °C | 67.79 GPa | |
550.0 °C | 66.02 GPa | |
600.0 °C | 64.16 GPa | |
Tensile strength | 20.0 °C | 460 - 610 MPa |
Yield strength | 20.0 °C | 300 MPa |
Yield strength Rp0.2 | 20.0 °C | 290 MPa |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Max service temperature, long | 400 - 550 °C | ||
Melting point | 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 46.3 W/(m·K) | |
100.0 °C | 47.1 W/(m·K) | ||
200.0 °C | 46.2 W/(m·K) | ||
300.0 °C | 44.1 W/(m·K) | ||
400.0 °C | 41.3 W/(m·K) | ||
500.0 °C | 38.6 W/(m·K) | ||
600.0 °C | 35.9 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 12.8 mm²/s | |
100.0 °C | 12.1 mm²/s | ||
200.0 °C | 11.1 mm²/s | ||
300.0 °C | 10 mm²/s | ||
400.0 °C | 8.8 mm²/s | ||
500.0 °C | 7.4 mm²/s | ||
600.0 °C | 4.7 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.25E-7 Ω·m |
50.0 °C | 2.41E-7 Ω·m | |
100.0 °C | 2.72E-7 Ω·m | |
150.0 °C | 3.04E-7 Ω·m | |
200.0 °C | 3.42E-7 Ω·m | |
250.0 °C | 3.83E-7 Ω·m | |
300.0 °C | 4.26E-7 Ω·m | |
350.0 °C | 4.74E-7 Ω·m | |
400.0 °C | 5.26E-7 Ω·m | |
450.0 °C | 5.83E-7 Ω·m | |
500.0 °C | 6.4E-7 Ω·m | |
550.0 °C | 7.04E-7 Ω·m | |
600.0 °C | 7.73E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Aluminium | 0.02 % |
Carbon | 0.1 - 0.18 % |
Chromium | 0.3 - 0.6 % |
Manganese | 0.4 - 0.7 % |
Molybdenum | 0.5 - 0.7 % |
Phosphorus | 0.03 % |
Silicon | 0.4 % |
Sulfur | 0.01 - 0.015 % |
Tin | 0.03 % |
Vanadium | 0.22 - 0.28 % |
Metal
- EN 10222-3 Grade 12Ni14 – Normalized & Tempered Nickel Alloy for Cryogenic Applications
- EN 10222-3 Grade 13MnNi6-3: Normalized & Tempered Cryogenic Alloy for Pressure Vessels
- EN 10250-2 Grade C30 Steel – Normalized & Tempered (+NT) for High Ductility Applications
- EN 10250‑2 Grade C40 Steel – Normalized & Tempered (NT) – Key Properties & Applications
- EN 10250-2 Grade C50 Normalized & Tempered Steel – High Strength & Abrasion Resistance
- EN 10222-2 Grade X10CrMoVNb9-1: Normalized & Tempered High-Temperature Stainless Steel for Pressure Vessels
- EN 10222-2: Grade 13CrMo4-5 (Normalized & Tempered) – Industrial Grade Steel for Pressure Vessels
- EN 10222-2 Grade P245GH – High-Temperature Steel, Normalized & Tempered (NT)