EN 10250‑2 Grade C22 Steel – Normalized & Tempered (NT) for High‑Performance Vehicle Components

Steel C22 is suitable for low strained parts of small heat-treatment sections in vehicle and machine engineering (e.g. piston rods, gear wheels).

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.83 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

217 GPa

20.0 °C

211.35 - 212 GPa

100.0 °C

206.1 - 207 GPa

200.0 °C

198.84 - 199 GPa

300.0 °C

191.11 - 192 GPa

400.0 °C

182.92 - 184 GPa

500.0 °C

172.88 - 175 GPa

600.0 °C

164 GPa

Elongation

20.0 °C

25 %

Poisson's ratio

20.0 °C

0.29 [-]

100.0 °C

0.29 [-]

200.0 °C

0.29 [-]

300.0 °C

0.3 [-]

400.0 °C

0.3 [-]

500.0 °C

0.31 [-]

Shear modulus

20.0 °C

82.19 GPa

100.0 °C

80.03 GPa

200.0 °C

76.94 GPa

300.0 °C

73.69 GPa

400.0 °C

70.14 GPa

500.0 °C

66.12 GPa

Tensile strength

20.0 °C

410 MPa

Yield strength

20.0 °C

210 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.08E-5 1/K

20.0 °C

1.19E-5 1/K

100.0 °C

1.25E-5 1/K

200.0 °C

1.3E-5 1/K

300.0 °C

1.36E-5 1/K

400.0 °C

1.41E-5 1/K

500.0 °C

1.45E-5 1/K

600.0 °C

1.49E-5 1/K

Max service temperature

500 °C

Typical for Carbon Steel

Melting point

1480 - 1526 °C

Typical for Low Carbon Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

20.0 °C

461 J/(kg·K)

100.0 °C

479 J/(kg·K)

200.0 °C

499 J/(kg·K)

300.0 °C

517 J/(kg·K)

400.0 °C

536 J/(kg·K)

500.0 °C

558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Thermal conductivity

-100.0 °C

37.6 W/(m·K)

20.0 °C

42.2 W/(m·K)

100.0 °C

43.2 W/(m·K)

200.0 °C

42.9 W/(m·K)

300.0 °C

41.2 W/(m·K)

400.0 °C

39.1 W/(m·K)

500.0 °C

36.6 W/(m·K)

600.0 °C

34.1 W/(m·K)

Thermal diffusivity

-100.0 °C

12.9 mm²/s

20.0 °C

11.7 mm²/s

100.0 °C

11.2 mm²/s

200.0 °C

10.3 mm²/s

300.0 °C

9.4 mm²/s

400.0 °C

8.3 mm²/s

500.0 °C

7.1 mm²/s

600.0 °C

5.7 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

-100.0 °C

1.82E-7 Ω·m

20.0 °C

2.47E-7 Ω·m

100.0 °C

2.96E-7 Ω·m

200.0 °C

3.68E-7 Ω·m

300.0 °C

4.55E-7 Ω·m

400.0 °C

5.56E-7 Ω·m

500.0 °C

6.75E-7 Ω·m

600.0 °C

8.13E-7 Ω·m

Magnetic

PropertyValueComment

Curie temperature

770 °C

Typical for Low Carbon Steel

Chemical properties

PropertyValue

Carbon

0.17 - 0.24 %

Chromium

0.4 %

Manganese

0.4 - 0.7 %

Molybdenum

0.1 %

Nickel

0.4 %

Phosphorus

0.05 %

Silicon

0.4 %

Sulfur

0.045 %


Metal

  1. EN 10250-2 Grade C30 Steel – Normalized & Tempered (+NT) for High Ductility Applications
  2. EN 10250‑2 Grade C40 Steel – Normalized & Tempered (NT) – Key Properties & Applications
  3. EN 10250-2 Grade C50 Normalized & Tempered Steel – High Strength & Abrasion Resistance
  4. EN 10250-2 Grade 28Mn6 Steel – Normalized & Tempered for High-Performance Applications
  5. EN 10250‑2 Grade C35E – Normalized & Tempered Steel for High-Performance Applications
  6. EN 10250-2 Grade C45E: Normalized & Tempered Steel for Heavy‑Duty Applications
  7. EN 10250-2 Grade C55E: Normalized & Tempered Steel for Heavy-Duty Applications
  8. EN 10250-2 Grade C60E Steel – Normalized & Tempered (NT) – High-Performance Industrial Alloy
  9. EN 10250-2 Grade C35 Steel – Normalized & Tempered (NT)
  10. EN 10250-2 C45 Steel – Normalized & Tempered Grade for Automotive & Machinery Applications