EN 10250-2 Grade 28Mn6 Steel – Normalized & Tempered for High-Performance Applications
Steel 28Mn6 is usable for lower strained weldable parts in vehicle, engine and machine engineering (e.g. cardan shafts, camshafts, gear wheels).
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.82 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Elongation | 20.0 °C | 17 - 18 % | |
Elongation, transverse | 20.0 °C | 11 - 13 % | |
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Manganese Steel |
Tensile strength | 20.0 °C | 540 - 600 MPa | |
Tensile strength, transverse | 20.0 °C | 540 - 590 MPa | |
Yield strength | 20.0 °C | 260 - 310 MPa | |
Yield strength, transverse | 20.0 °C | 260 - 390 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K | ||
Melting point | 1382 - 1529 °C | Typical for Manganese Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 48 W/(m·K) | |
100.0 °C | 48.9 W/(m·K) | ||
200.0 °C | 47.5 W/(m·K) | ||
300.0 °C | 44.7 W/(m·K) | ||
400.0 °C | 41.6 W/(m·K) | ||
500.0 °C | 38.6 W/(m·K) | ||
600.0 °C | 35.5 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 13.3 mm²/s | |
100.0 °C | 12.6 mm²/s | ||
200.0 °C | 11.5 mm²/s | ||
300.0 °C | 10.2 mm²/s | ||
400.0 °C | 8.9 mm²/s | ||
500.0 °C | 7.5 mm²/s | ||
600.0 °C | 6 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.17E-7 Ω·m |
100.0 °C | 2.62E-7 Ω·m | |
200.0 °C | 3.32E-7 Ω·m | |
300.0 °C | 4.2E-7 Ω·m | |
400.0 °C | 5.23E-7 Ω·m | |
500.0 °C | 6.41E-7 Ω·m | |
600.0 °C | 7.8E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.25 - 0.32 % |
Chromium | 0.4 % |
Manganese | 1.3 - 1.65 % |
Molybdenum | 0.1 % |
Nickel | 0.4 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.035 % |
Metal
- EN 10250-2 Grade C30 Steel – Normalized & Tempered (+NT) for High Ductility Applications
- EN 10250‑2 Grade C40 Steel – Normalized & Tempered (NT) – Key Properties & Applications
- EN 10250-2 Grade C50 Normalized & Tempered Steel – High Strength & Abrasion Resistance
- EN 10250‑2 Grade C35E – Normalized & Tempered Steel for High-Performance Applications
- EN 10250-2 Grade C45E: Normalized & Tempered Steel for Heavy‑Duty Applications
- EN 10250-2 Grade C55E: Normalized & Tempered Steel for Heavy-Duty Applications
- EN 10250-2 Grade C60E Steel – Normalized & Tempered (NT) – High-Performance Industrial Alloy
- EN 10250-2 Grade C35 Steel – Normalized & Tempered (NT)
- EN 10250‑2 Grade C22 Steel – Normalized & Tempered (NT) for High‑Performance Vehicle Components
- EN 10250-2 C45 Steel – Normalized & Tempered Grade for Automotive & Machinery Applications