EN 10132-4 Grade 80CrV2 Steel: Quenched & Tempered (QT) – High-Performance Spring Strip
The steel 80CrV2 is used as cold rolled strip for springs and special applications in thicknesses of up to 6 mm and as tempered cold strip in thicknesses from 0.30 to 3.00 mm.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.81 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Hardness, Rockwell C | 20.0 °C | 38.5 - 52.5 [-] | |
Hardness, Vickers | 20.0 °C | 370 - 605 [-] | |
Poisson's ratio | 20.0 °C | 0.28 [-] | |
Shear modulus | 23.0 °C | 79 GPa | Typical for Tool And Machining Steel |
Tensile strength | 20.0 °C | 1200 - 1800 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Melting point | 1370 - 1425 °C | Typical for Tool And Machining Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 39.6 W/(m·K) | |
100.0 °C | 41.6 W/(m·K) | ||
200.0 °C | 41.8 W/(m·K) | ||
300.0 °C | 40.3 W/(m·K) | ||
400.0 °C | 38.2 W/(m·K) | ||
500.0 °C | 36 W/(m·K) | ||
600.0 °C | 33.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11 mm²/s | |
100.0 °C | 10.8 mm²/s | ||
200.0 °C | 10.1 mm²/s | ||
300.0 °C | 9.2 mm²/s | ||
400.0 °C | 8.1 mm²/s | ||
500.0 °C | 7 mm²/s | ||
600.0 °C | 5.7 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.63E-7 Ω·m |
100.0 °C | 3.08E-7 Ω·m | |
200.0 °C | 3.78E-7 Ω·m | |
300.0 °C | 4.66E-7 Ω·m | |
400.0 °C | 5.69E-7 Ω·m | |
500.0 °C | 6.87E-7 Ω·m | |
600.0 °C | 8.26E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.75 - 0.85 % |
Chromium | 0.4 - 0.6 % |
Manganese | 0.3 - 0.5 % |
Molybdenum | 0.1 % |
Nickel | 0.4 % |
Phosphorus | 0.03 % |
Silicon | 0.15 - 0.35 % |
Sulfur | 0.025 % |
Vanadium | 0.15 - 0.25 % |
Metal
- EN 10132‑4 Grade 80CrV2 Quenched Steel (Q) – High‑Performance Spring & Cold‑Rolled Strip
- EN 10132-4 Grade 51CrV4 Quenched & Tempered Steel (QT) – High-Performance Cold-Rolled Strip
- EN 10132-4 Grade 102Cr6 Quenched & Tempered Steel – High Strength, Low Temperature Performance
- EN 10132-4 Grade C55S Quenched & Tempered Steel – Ideal for Springs & Cold-Rolled Strips
- EN 10132-4 Grade C60S – Premium Quenched & Tempered High‑Carbon Steel
- EN 10132-4 Grade C90S Quenched & Tempered Steel – High-Performance Spring Material
- EN 10132-4 Grade C100S: Quenched & Tempered Steel for Precision Springs and Cold‑Rolled Applications
- EN 10132‑4 Grade C85S Quenched & Tempered Steel – Premium Cold‑Rolled Strip for Springs & Thin Components
- EN 10132-4 Grade C125S Quenched & Tempered Steel – Precision Spring & Watch Industry Grade
- EN 10132-4 Grade C75S Quenched & Tempered Steel – High-Strength, High-Hardness Performance