DIN 5512-1 Grade S355J2G1W Steel – As-Rolled with Annealing (AR)
The steel is used for rail vehicle engineering acc. to the selected standard DIN 5512-1.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.84 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Elongation | 20.0 °C | 20 - 22 % | |
Elongation A80 | 20.0 °C | 16 - 18 % | |
Elongation A80, transverse | 20.0 °C | 14 - 16 % | |
Elongation, transverse | 20.0 °C | 18 - 20 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] | Typical for Steel |
Tensile strength | 20.0 °C | 490 - 680 MPa | |
Yield strength | 20.0 °C | 315 - 355 MPa | |
Thermal
| Property | Temperature | Value |
|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K |
20.0 °C | 1.19E-5 1/K | |
100.0 °C | 1.25E-5 1/K | |
200.0 °C | 1.3E-5 1/K | |
300.0 °C | 1.36E-5 1/K | |
400.0 °C | 1.41E-5 1/K | |
500.0 °C | 1.45E-5 1/K | |
600.0 °C | 1.49E-5 1/K | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) | |
Thermal conductivity | -100.0 °C | 46.5 W/(m·K) |
20.0 °C | 49.4 W/(m·K) | |
100.0 °C | 49.4 W/(m·K) | |
200.0 °C | 47.8 W/(m·K) | |
300.0 °C | 45.1 W/(m·K) | |
400.0 °C | 41.8 W/(m·K) | |
500.0 °C | 38.6 W/(m·K) | |
600.0 °C | 35.3 W/(m·K) | |
Thermal diffusivity | -100.0 °C | 15.9 mm²/s |
20.0 °C | 13.7 mm²/s | |
100.0 °C | 12.7 mm²/s | |
200.0 °C | 11.5 mm²/s | |
300.0 °C | 10.2 mm²/s | |
400.0 °C | 8.9 mm²/s | |
500.0 °C | 7.4 mm²/s | |
600.0 °C | 5.8 mm²/s | |
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | -100.0 °C | 1.47E-7 Ω·m |
20.0 °C | 2.11E-7 Ω·m | |
100.0 °C | 2.59E-7 Ω·m | |
200.0 °C | 3.3E-7 Ω·m | |
300.0 °C | 4.16E-7 Ω·m | |
400.0 °C | 5.2E-7 Ω·m | |
500.0 °C | 6.41E-7 Ω·m | |
600.0 °C | 7.85E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.16 % |
Chromium | 0.4 - 0.8 % |
Copper | 0.25 - 0.55 % |
Manganese | 0.5 - 1 % |
Molybdenum | 0.3 % |
Nickel | 0.65 % |
Phosphorus | 0.04 % |
Silicon | 0.5 % |
Sulfur | 0.035 % |
Zirconium | 0.15 % |
Metal
- EN 10025-5 S355J2G1W Steel – As‑Rolled with Enhanced Atmospheric Corrosion Resistance
- DIN 5512-1 Grade S235J2G3C Steel – As-Rolled Condition (AR) – Technical Specs & Applications
- EN 10025 S235J2G4C Steel – As-Rolled Grade for Dynamic Structures
- EN 10025 S235JRC Steel – As‑Rolled (AR) Grade for Construction
- EN 10025 Grade S235JRG1: As-Rolled Steel for Cold-Forming and Welding
- EN 10025 Grade S355J2G4C - High-Strength As-Rolled Steel (+AR) for Dynamic Load Applications
- EN 10025 S355K2G4C Steel – High-Tensile, Fine-Grained (As-Rolled + AR)
- EN 10025 Grade S275J0C – As‑Rolled Steel (+AR) for Cold Forming Applications
- EN 10025 S275JRC Steel – As-Rolled (+AR) for Cold Forming & Drawing
- EN 10025 Grade S235J0C – As-Rolled Condition (+AR) – High‑Performance Low‑Carbon Steel