EN 10025-5 S355J2G1W Steel – As‑Rolled with Enhanced Atmospheric Corrosion Resistance
The material S355J2G1W with improved atmospheric corrosion resistance (by generation of an conversion coating) has a minimum yield strength of 355 N/mm². It is applicated for welded, screwed and riveted constructions, e.g. structural engineering, bridge building, tank construction, exhaust systems, vehicle construction, toolbuilding. The atmospheric load have to consider (SEW 087, Guideline 007 of the Deutscher Ausschuss für Stahlbau and paragraph 2.5 of TA-Luft 1986). The unhindered generation of the conversion coating have to be considered in the construction and building process. The grid rate have to considered in the dimensioning process. An conventional surface protection is recommend at polluted air and necessary at long-time water wetting, constant wetness or close to the sea. Unweathered areas with condensate generation have to be adequate ventilated. Before welding the coating have to be removed in a distance of 10 - 20 mm from the welding edge. With increasing thickness, strength and carbon equivalent the occurence of cold cracks in the welding zone is possible. The recommendation of the EURONORM Information No. 2 (EN 1011) have to considered. Application limit: An notch impact energy of 27 J at -20 deg. is guaranteed.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.84 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Elongation | 20.0 °C | 20 - 22 % | |
Elongation A80 | 20.0 °C | 16 - 18 % | |
Elongation A80, transverse | 20.0 °C | 14 - 16 % | |
Elongation, transverse | 20.0 °C | 18 - 20 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] | Typical for Steel |
Tensile strength | 20.0 °C | 490 - 680 MPa | |
Yield strength | 20.0 °C | 315 - 355 MPa | |
Thermal
| Property | Temperature | Value |
|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K |
20.0 °C | 1.19E-5 1/K | |
100.0 °C | 1.25E-5 1/K | |
200.0 °C | 1.3E-5 1/K | |
300.0 °C | 1.36E-5 1/K | |
400.0 °C | 1.41E-5 1/K | |
500.0 °C | 1.45E-5 1/K | |
600.0 °C | 1.49E-5 1/K | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) | |
Thermal conductivity | -100.0 °C | 46.5 W/(m·K) |
20.0 °C | 49.4 W/(m·K) | |
100.0 °C | 49.4 W/(m·K) | |
200.0 °C | 47.8 W/(m·K) | |
300.0 °C | 45.1 W/(m·K) | |
400.0 °C | 41.8 W/(m·K) | |
500.0 °C | 38.6 W/(m·K) | |
600.0 °C | 35.3 W/(m·K) | |
Thermal diffusivity | -100.0 °C | 15.9 mm²/s |
20.0 °C | 13.7 mm²/s | |
100.0 °C | 12.7 mm²/s | |
200.0 °C | 11.5 mm²/s | |
300.0 °C | 10.2 mm²/s | |
400.0 °C | 8.9 mm²/s | |
500.0 °C | 7.4 mm²/s | |
600.0 °C | 5.8 mm²/s | |
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | -100.0 °C | 1.47E-7 Ω·m |
20.0 °C | 2.11E-7 Ω·m | |
100.0 °C | 2.59E-7 Ω·m | |
200.0 °C | 3.3E-7 Ω·m | |
300.0 °C | 4.16E-7 Ω·m | |
400.0 °C | 5.2E-7 Ω·m | |
500.0 °C | 6.41E-7 Ω·m | |
600.0 °C | 7.85E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.16 % |
Chromium | 0.4 - 0.8 % |
Copper | 0.25 - 0.55 % |
Manganese | 0.5 - 1 % |
Molybdenum | 0.3 % |
Nickel | 0.65 % |
Phosphorus | 0.04 % |
Silicon | 0.5 % |
Sulfur | 0.035 % |
Zirconium | 0.15 % |
Metal
- DIN 5512-1 Grade S355J2G1W Steel – As-Rolled with Annealing (AR)
- DIN 5512-1 Grade S235J2G3C Steel – As-Rolled Condition (AR) – Technical Specs & Applications
- EN 10025 S235J2G4C Steel – As-Rolled Grade for Dynamic Structures
- EN 10025 S235JRC Steel – As‑Rolled (AR) Grade for Construction
- EN 10025 Grade S235JRG1: As-Rolled Steel for Cold-Forming and Welding
- EN 10025 Grade S355J2G4C - High-Strength As-Rolled Steel (+AR) for Dynamic Load Applications
- EN 10025 S355K2G4C Steel – High-Tensile, Fine-Grained (As-Rolled + AR)
- EN 10025 Grade S275J0C – As‑Rolled Steel (+AR) for Cold Forming Applications