EN 1561 Grade GJL-200: Standard Cast Condition for High-Performance Applications
EN-GJL-200 is used for various molded parts, precision castings, furnaces as well as for radiators.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.15 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Compressive yield strength | 20.0 °C | 636 - 954 MPa | |
Compressive yield strength, 0.1% | 20.0 °C | 260 MPa | |
Elastic modulus | 20.0 °C | 88 - 113 GPa | |
Elongation | 20.0 °C | 0.3 - 0.8 % | |
Flexural strength | 20.0 °C | 346 - 519 MPa | |
Plane-Strain Fracture Toughnes | 20.0 °C | 17 MPa·√m | |
Poisson's ratio | 20.0 °C | 0.25 - 0.26 [-] | |
Shear modulus | 23.0 °C | 41 GPa | Typical for Cast Iron |
Shear strength | 20.0 °C | 230 MPa | |
Tensile strength | 20.0 °C | 160 - 300 MPa | |
100.0 °C | 200 MPa | ||
200.0 °C | 190 MPa | ||
300.0 °C | 200 MPa | ||
400.0 °C | 210 MPa | ||
500.0 °C | 160 MPa | ||
600.0 °C | 110 MPa | ||
Torsion Strength | 20.0 °C | 272 - 408 MPa | |
Yield strength Rp0.1 | 20.0 °C | 130 - 195 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1E-5 1/K | |
100.0 °C | 1.05E-5 1/K | ||
200.0 °C | 1.17E-5 1/K | ||
300.0 °C | 1.2E-5 1/K | ||
400.0 °C | 1.3E-5 1/K | ||
500.0 °C | 1.3E-5 1/K | ||
600.0 °C | 1.3E-5 1/K | ||
Melting point | 1127 - 1204 °C | Typical for Grey Cast Iron | |
Specific heat capacity | 200.0 °C | 460 J/(kg·K) | |
600.0 °C | 535 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 54 W/(m·K) | |
100.0 °C | 50 W/(m·K) | ||
200.0 °C | 49 W/(m·K) | ||
300.0 °C | 48 W/(m·K) | ||
400.0 °C | 47 W/(m·K) | ||
500.0 °C | 46 W/(m·K) | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 7E-7 - 7.7E-7 Ω·m |
Technological properties
| Property | ||
|---|---|---|
| Processing methods | sand casting | |
Metal
- EN 13835 Grade GGG-Ni 22 – Premium Nickel-Containing Cast Iron
- EN 13835: GGG‑NiMn 23/4 Cast Iron – High‑Strain, Cryogenic‑Grade Material
- EN 13835 GGL‑NiCr 30/3: High‑Temperature, Corrosion‑Resistant Cast Iron for Pumps, Boilers, and Turbochargers
- DIN 17730 Grade G‑Ni93C: Low‑Galling, Corrosion‑Resistant Cast Material for Food‑Grade and Industrial Applications
- EN 12844 Grade G‑ZnAl4Cu3: Advanced Casting Alloy for High‑Strength Applications
- EN 12844: Grade G‑ZnAl6Cu1 Casting Specifications & Performance
- EN 1561 GJL-150: Comprehensive Cast Condition Specifications
- EN 1561 Grade GJL-250 Cast – Key Properties & Applications
- EN 1561 Grade GJL‑300: Standard Cast Material for Industrial Applications
- EN 1561 GJL-350 Cast Steel: Properties & Applications