EN 10132-3 Grade C50E Quenched & Tempered Cold-Rolled Strip – High Strength, Precise Thicknesses

Cold-rolled narrow strip made of the mild steel C50E will be delivered in thicknesses up to 6 mm for quenching and tempering and for quenched and tempered cold strip in thicknesses between 0.3 mm and 3.0 mm in following conditions: - soft annealed or soft annealed and little rerolled (+A or +LC), - cold rolled (+CR), - quenched and tempered (+QT). The delivery condition annealed to globular carbides (+AC) can be agreed.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.8 - 7.85 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

217 GPa

20.0 °C

210 - 212 GPa

100.0 °C

205 - 207 GPa

200.0 °C

195 - 199 GPa

300.0 °C

185 - 192 GPa

400.0 °C

175 - 184 GPa

500.0 °C

175 GPa

600.0 °C

164 GPa

Hardness, Rockwell C

20.0 °C

33 - 49.5 [-]

Hardness, Vickers

20.0 °C

325 - 505 [-]

Poisson's ratio

23.0 °C

0.29 [-]

Typical for Medium Carbon Steel

Shear modulus

20.0 °C

81 GPa

Tensile strength

20.0 °C

1050 - 1650 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.08E-5 1/K

20.0 °C

1.19E-5 1/K

100.0 °C

1.11E-5 - 1.25E-5 1/K

200.0 °C

1.21E-5 - 1.3E-5 1/K

300.0 °C

1.29E-5 - 1.36E-5 1/K

400.0 °C

1.35E-5 - 1.41E-5 1/K

500.0 °C

1.45E-5 1/K

600.0 °C

1.49E-5 1/K

Max service temperature

500 °C

Typical for Carbon Steel

Melting point

1380 - 1514 °C

Typical for Medium Carbon Steel

Specific heat capacity

-100.0 °C

423 J/(kg·K)

20.0 °C

460 - 461 J/(kg·K)

100.0 °C

479 J/(kg·K)

200.0 °C

499 J/(kg·K)

300.0 °C

517 J/(kg·K)

400.0 °C

536 J/(kg·K)

500.0 °C

558 J/(kg·K)

600.0 °C

587 J/(kg·K)

Thermal conductivity

20.0 °C

41.7 - 52 W/(m·K)

100.0 °C

43.4 - 50.6 W/(m·K)

200.0 °C

43.2 - 48.1 W/(m·K)

300.0 °C

41.4 - 45.7 W/(m·K)

400.0 °C

39.1 W/(m·K)

500.0 °C

36.7 W/(m·K)

600.0 °C

34.1 W/(m·K)

Thermal diffusivity

20.0 °C

11.6 mm²/s

100.0 °C

11.3 mm²/s

200.0 °C

10.5 mm²/s

300.0 °C

9.5 mm²/s

400.0 °C

8.3 mm²/s

500.0 °C

7.1 mm²/s

600.0 °C

5.8 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

1.2E-7 - 2.5E-7 Ω·m

100.0 °C

2.95E-7 Ω·m

200.0 °C

3.65E-7 Ω·m

300.0 °C

4.53E-7 Ω·m

400.0 °C

5.56E-7 Ω·m

500.0 °C

6.74E-7 Ω·m

600.0 °C

8.13E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.47 - 0.55 %

Chromium

0.4 %

Manganese

0.6 - 0.9 %

Molybdenum

0.1 %

Nickel

0.4 %

Phosphorus

0.04 %

Silicon

0.4 %

Sulfur

0.035 %


Metal

  1. EN 10137-2 Grade S890QL – High-Strength Quenched & Tempered Steel for Heavy-Duty Applications
  2. EN 10137-3 Grade S500A: Quenched & Tempered Fine‑Grained Steel for Structural Applications
  3. EN 10083-1 Grade 51CrV4: Quenched & Tempered Steel (QT)
  4. EN 10132-3: 42CrMo4 Quenched & Tempered Alloy Steel – Premium Cold-Rolled Strips
  5. Premium 34CrMo4 Cold Rolled Strip – EN 10132‑3 Quenched & Tempered (QT)
  6. EN 10132-3 Grade C50E Quenched Cold-Rolled Strip – Premium Mild Steel for Advanced Applications
  7. EN 10132-3: 25CrMo4 Quenched & Tempered Cold-Rolled Strip – Precision Steel for Industrial Applications
  8. EN 10132-3 Grade C60E – High-Quality Quenched & Tempered Cold-Rolled Steel
  9. EN 10132-3 Grade C55E: Quenched & Tempered Cold‑Rolled Steel for High‑Performance Applications
  10. EN 10083‑2 Grade C50E: High‑Performance Quenched & Tempered Steel for Heavy Forged Parts