EN 10132-3: 25CrMo4 Quenched & Tempered Cold-Rolled Strip – Precision Steel for Industrial Applications
Cold-rolled narrow strip made of the alloy steel 25CrMo4 will be delivered in thicknesses up to 6 mm for quenching and tempering and for quenched and tempered cold strip in thicknesses between 0.3 mm and 3.0 mm in following conditions: - soft annealed or soft annealed and little rerolled (+A or +LC), - cold rolled (+CR), - quenched and tempered (+QT). The delivery condition annealed to globular carbides (+AC) can be agreed.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.83 - 7.85 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 210 - 212 GPa | ||
100.0 °C | 205 - 207 GPa | ||
200.0 °C | 195 - 199 GPa | ||
300.0 °C | 185 - 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Hardness, Rockwell C | 20.0 °C | 31.5 - 44 [-] | |
Hardness, Vickers | 20.0 °C | 305 - 435 [-] | |
Poisson's ratio | 23.0 °C | 0.29 [-] | Typical for Chromium Molybdenum Steel |
Shear modulus | 20.0 °C | 81 GPa | |
Tensile strength | 20.0 °C | 990 - 1400 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K | ||
100.0 °C | 1.11E-5 - 1.21E-5 1/K | ||
200.0 °C | 1.21E-5 - 1.27E-5 1/K | ||
300.0 °C | 1.29E-5 - 1.32E-5 1/K | ||
400.0 °C | 1.35E-5 - 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K | ||
Max service temperature, long | 0 - 200 °C | ||
Melting point | 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 460 - 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41 - 50 W/(m·K) | |
100.0 °C | 42.7 W/(m·K) | ||
200.0 °C | 42.8 W/(m·K) | ||
300.0 °C | 41.6 W/(m·K) | ||
400.0 °C | 39.9 W/(m·K) | ||
500.0 °C | 37.8 W/(m·K) | ||
600.0 °C | 35.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.4 mm²/s | |
100.0 °C | 11 mm²/s | ||
200.0 °C | 10.3 mm²/s | ||
300.0 °C | 9.5 mm²/s | ||
400.0 °C | 8.5 mm²/s | ||
500.0 °C | 7.3 mm²/s | ||
600.0 °C | 6 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 1.8E-7 - 2.54E-7 Ω·m |
100.0 °C | 3E-7 Ω·m | |
200.0 °C | 3.69E-7 Ω·m | |
300.0 °C | 4.51E-7 Ω·m | |
400.0 °C | 5.45E-7 Ω·m | |
500.0 °C | 6.54E-7 Ω·m | |
600.0 °C | 7.78E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.22 - 0.29 % |
Chromium | 0.9 - 1.2 % |
Manganese | 0.6 - 0.9 % |
Molybdenum | 0.15 - 0.3 % |
Phosphorus | 0.04 % |
Silicon | 0.4 % |
Sulfur | 0.035 % |
Metal
- EN 10132-3: 42CrMo4 Quenched & Tempered Alloy Steel – Premium Cold-Rolled Strips
- Premium 34CrMo4 Cold Rolled Strip – EN 10132‑3 Quenched & Tempered (QT)
- EN 10297-1 Grade 25CrMo4 Quenched & Tempered Steel – Properties & Applications
- EN 10132-3 Grade C60E – High-Quality Quenched & Tempered Cold-Rolled Steel
- EN 10132-3 Grade C50E Quenched & Tempered Cold-Rolled Strip – High Strength, Precise Thicknesses
- EN 10132-3 Grade C55E: Quenched & Tempered Cold‑Rolled Steel for High‑Performance Applications
- EN 10269 Grade 25CrMo4 Quenched & Tempered: Premium High‑Strength Steel
- EN 10263-4 Grade 25CrMo4 Quenched & Tempered Steel – High Strength, Cold-Formable
- EN 10083-1 Grade 25CrMo4 Quenched & Tempered Steel: High Strength & Ductility for Automotive & Engine Components
- EN 10216-2 Grade 25CrMo4 Quenched & Tempered Seamless Tubes for High‑Temperature Applications