Pink Sheets Grade 319.0 T6 – Comprehensive Material Specifications
Properties
General
| Property | Value | Condition |
|---|---|---|
Density | 3.0 g/cm³ | T6 |
Mechanical
| Property | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|
Compressive yield strength | 172.0 - 193.0 MPa | T6 | |||
Elastic modulus | 74 GPa | T6 | |||
78.0 GPa | T6 | ||||
Elongation | 1.5 - 2.0 % | T6 | Sand cast, elongation in 50 mm | ||
1.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | A100 | |
1.8 % | T6 | ||||
Fatigue strength | 76.0 - 83.0 MPa | T6 | for 5x10⁸ cycles, R.R. Moore type test | ||
Hardness, Brinell | 80.0 - 95.0 [-] | T6 | 500 kg load, 10 mm b | ||
80.0 [-] | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
Poisson's ratio | 0.33 [-] | T6 | |||
Shear modulus | 28.0 GPa | T6 | |||
Shear strength | 200.0 - 220.0 MPa | T6 | |||
Tensile strength | 215.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
250.0 MPa | T6 | ||||
250 MPa | T6 | Sand cast | |||
Yield strength | 140.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 |
160.0 MPa | T6 | ||||
164 MPa | T6 | Sand cast, RP02 |
Thermal
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Coefficient of thermal expansion | 2.3e-05 1/K | T6 | ||
Melting point | 510.0 - 607.0 °C | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
540.0 °C | T6 | |||
Specific heat capacity | 860.0 J/(kg·K) | T6 | ||
Thermal conductivity | 110.0 W/(m·K) | T6 |
Electrical
| Property | Value | Condition | Comment |
|---|---|---|---|
Electrical resistivity | 6.39e-08 Ω·m | T6 | Typical values |
Chemical properties
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Aluminium | 85.8 - 91.5 % | T6 | ||
Copper | 3.0 - 4.0 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Iron | 1.0 % | T6 | ||
1.00 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Magnesium | 0.1 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Manganese | 0.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Nickel | 0.35 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Other | 0.5 % | T6 | ||
Silicon | 5.5 - 6.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titanium | 0.25 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zinc | 1.0 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Metal
- Pink Sheets Grade 242.0 O – Comprehensive Material Properties & Standards
- Comprehensive Mechanical Properties of Pink Sheets Grade 319.0 T5 Alloy
- Pink Sheets 201.0 T7: High-Performance Mechanical Properties
- T61 Pink Sheets Grade 242.0 – Detailed Mechanical Properties
- Pink Sheets Grade 201.0 T6: Comprehensive Mechanical Property Data
- Pink Sheets Grade 355.0 T71 – Comprehensive Mechanical Properties & Performance Data
- Pink Sheets Grade 355.0 T6: Comprehensive Mechanical Properties & Standards
- Pink Sheets Grade 356.0 T6: Premium Alloy for Superior Mechanical Strength
- Comprehensive Overview of Pink Sheets Grade 319.0 F – Properties & Standards
- Pink Sheets Grade 356.0 T7: Comprehensive Material Properties & Standards