Pink Sheets Grade 356.0 T7: Comprehensive Material Properties & Standards
Properties
General
| Property | Value | Condition |
|---|---|---|
Density | 2.7 g/cm³ | T7 |
Mechanical
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Compressive yield strength | 165.0 - 214.0 MPa | T7 | ||||
Elastic modulus | 72.0 GPa | T7 | ||||
72.4 GPa | T7 | |||||
Elongation | -195 °C | 2 % | T7 | Sand cast, elongation in 50 mm | ||
-80 °C | 2 % | T7 | Sand cast, elongation in 50 mm | |||
-28 °C | 2 % | T7 | Sand cast, elongation in 50 mm | |||
3.0 % | T7 | Pink Sheets, ASTM B26 | Casting | A100 | ||
3.4 % | T7 | |||||
24 °C | 2 % | T7 | Sand cast, elongation in 50 mm | |||
100 °C | 2 % | T7 | Sand cast, elongation in 50 mm | |||
150 °C | 6 % | T7 | Sand cast, elongation in 50 mm | |||
205 °C | 18 % | T7 | Sand cast, elongation in 50 mm | |||
260 °C | 35 % | T7 | Sand cast, elongation in 50 mm | |||
315 °C | 60 % | T7 | Sand cast, elongation in 50 mm | |||
371 °C | 80 % | T7 | Sand cast, elongation in 50 mm | |||
Fatigue strength | 62.0 - 76.0 MPa | T7 | for 5x10⁸ cycles, R.R. Moore type test | |||
Hardness, Brinell | 60.0 [-] | T7 | Pink Sheets, ASTM B26 | Casting | ||
70.0 - 75.0 [-] | T7 | 500 kg load, 10 mm b | ||||
75.0 [-] | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
Poisson's ratio | 0.33 [-] | T7 | ||||
Shear modulus | 27.2 GPa | T7 | ||||
Shear strength | 165 MPa | T7 | ||||
Tensile strength | -195 °C | 283 MPa | T7 | Sand cast | ||
-80 °C | 248 MPa | T7 | Sand cast | |||
-28 °C | 235 MPa | T7 | Sand cast | |||
170.0 MPa | T7 | Pink Sheets, ASTM B26 | Casting | |||
215.0 MPa | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
230.0 MPa | T7 | |||||
24 °C | 235 MPa | T7 | Sand cast | |||
100 °C | 207 MPa | T7 | Sand cast | |||
150 °C | 160 MPa | T7 | Sand cast | |||
205 °C | 83 MPa | T7 | Sand cast | |||
260 °C | 53 MPa | T7 | Sand cast | |||
315 °C | 28 MPa | T7 | Sand cast | |||
371 °C | 17 MPa | T7 | Sand cast | |||
Yield strength | -195 °C | 240 MPa | T7 | Sand cast, RP02 | ||
-80 °C | 220 MPa | T7 | Sand cast, RP02 | |||
-28 °C | 215 MPa | T7 | Sand cast, RP02 | |||
125.0 MPa | T7 | Pink Sheets, ASTM B26 | Casting | RP02 | ||
190.0 MPa | T7 | |||||
24 °C | 207 MPa | T7 | Sand cast, RP02 | |||
100 °C | 193 MPa | T7 | Sand cast, RP02 | |||
150 °C | 138 MPa | T7 | Sand cast, RP02 | |||
205 °C | 58 MPa | T7 | Sand cast, RP02 | |||
260 °C | 34 MPa | T7 | Sand cast, RP02 | |||
315 °C | 21 MPa | T7 | Sand cast, RP02 | |||
371 °C | 14 MPa | T7 | Sand cast, RP02 |
Thermal
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2.2e-05 1/K | T7 | ||||
Melting point | 557.0 - 613.0 °C | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
570.0 °C | T7 | |||||
Specific heat capacity | 970.0 J/(kg·K) | T7 | ||||
Thermal conductivity | 150.0 W/(m·K) | T7 | ||||
25 °C | 155 W/(m·K) | T7 | nominal value |
Electrical
| Property | Value | Condition | Comment |
|---|---|---|---|
Electrical conductivity | 24000000 S/m | T7 | Typical/Derived values |
Electrical resistivity | 4.3099999999999996e-08 Ω·m | T7 | Typical values |
Specific Electrical conductivity | 40.0 - 43.0 % IACS | T7 | Typical values |
Chemical properties
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Aluminium | 90.1 - 93.3 % | T7 | ||
Copper | 0.25 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Iron | 0.6 % | T7 | ||
0.60 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Magnesium | 0.2 - 0.45 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Manganese | 0.35 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Other | 0.15 % | T7 | ||
Silicon | 6.5 - 7.5 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titanium | 0.25 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zinc | 0.35 % | T7 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Metal
- Pink Sheets Grade 242.0 O – Comprehensive Material Properties & Standards
- Comprehensive Mechanical Properties of Pink Sheets Grade 319.0 T5 Alloy
- Pink Sheets 201.0 T7: High-Performance Mechanical Properties
- T61 Pink Sheets Grade 242.0 – Detailed Mechanical Properties
- Pink Sheets Grade 201.0 T6: Comprehensive Mechanical Property Data
- Pink Sheets Grade 319.0 T6 – Comprehensive Material Specifications
- T51 Pink Sheets Alloy – Grade 356.0 – Key Mechanical Properties
- Pink Sheets Grade 355.0 T6: Comprehensive Mechanical Properties & Standards
- Pink Sheets Grade 356.0 T6: Premium Alloy for Superior Mechanical Strength
- Comprehensive Overview of Pink Sheets Grade 319.0 F – Properties & Standards