Pink Sheets Grade 355.0 T6: Comprehensive Mechanical Properties & Standards
Properties
General
| Property | Value | Condition |
|---|---|---|
Density | 2.8 g/cm³ | T6 |
Mechanical
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Compressive yield strength | 179.0 - 186.0 MPa | T6 | ||||
Elastic modulus | 76.0 GPa | T6 | ||||
25 °C | 70.3 GPa | T6 | ||||
150 °C | 67.6 GPa | T6 | ||||
204 °C | 64.1 GPa | T6 | ||||
260 °C | 56.5 GPa | T6 | ||||
Elongation | 2.0 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | A100 | |
2.6 % | T6 | |||||
25 °C | 3 % | T6 | Sand cast, elongation in 50 mm | |||
150 °C | 1.5 % | T6 | Sand cast, elongation in 50 mm | |||
205 °C | 8 % | T6 | Sand cast, elongation in 50 mm | |||
260 °C | 16 % | T6 | Sand cast, elongation in 50 mm | |||
315 °C | 36 % | T6 | Sand cast, elongation in 50 mm | |||
Fatigue strength | 62.0 - 70.0 MPa | T6 | for 5x10⁸ cycles, R.R. Moore type test | |||
Hardness, Brinell | 80.0 - 90.0 [-] | T6 | 500 kg load, 10 mm b | |||
80.0 [-] | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
Poisson's ratio | 0.33 [-] | T6 | ||||
Shear modulus | 26.2 GPa | T6 | ||||
Shear strength | 193.0 - 234.0 MPa | T6 | ||||
Tensile strength | 220.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
260.0 MPa | T6 | |||||
25 °C | 240 MPa | T6 | Sand cast | |||
150 °C | 230 MPa | T6 | Sand cast | |||
205 °C | 115 MPa | T6 | Sand cast | |||
260 °C | 65 MPa | T6 | Sand cast | |||
315 °C | 40 MPa | T6 | Sand cast | |||
Yield strength | 140.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 | |
170.0 MPa | T6 | |||||
25 °C | 170 MPa | T6 | Sand cast, RP02 | |||
150 °C | 170 MPa | T6 | Sand cast, RP02 | |||
205 °C | 90 MPa | T6 | Sand cast, RP02 | |||
260 °C | 35 MPa | T6 | Sand cast, RP02 | |||
315 °C | 20 MPa | T6 | Sand cast, RP02 |
Thermal
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2.3e-05 1/K | T6 | ||||
100 °C | 0.0000223 1/K | T6 | nominal value between 20°C and the mentioned temperature | |||
300 °C | 0.0000247 1/K | T6 | nominal value between 20°C and the mentioned temperature | |||
Melting point | 546.0 - 621.0 °C | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
560.0 °C | T6 | |||||
Specific heat capacity | 880.0 J/(kg·K) | T6 | ||||
100 °C | 960 J/(kg·K) | T6 | derived value | |||
Thermal conductivity | 150.0 W/(m·K) | T6 | ||||
25 °C | 142 W/(m·K) | T6 | nominal value |
Electrical
| Property | Value | Condition | Comment |
|---|---|---|---|
Electrical conductivity | 22619999.999999996 S/m | T6 | Typical/Derived values |
Electrical resistivity | 4.42e-08 Ω·m | T6 | Typical values |
Specific Electrical conductivity | 39 % IACS | T6 | Typical values |
Chemical properties
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Aluminium | 90.3 - 94.1 % | T6 | ||
Chromium | 0.25 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Copper | 1.0 - 1.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Iron | 0.6 % | T6 | ||
0.60 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Magnesium | 0.4 - 0.6 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Manganese | 0.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Other | 0.15 % | T6 | ||
Silicon | 4.5 - 5.5 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Titanium | 0.25 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Zinc | 0.35 % | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting |
Metal
- Pink Sheets Grade 242.0 O – Comprehensive Material Properties & Standards
- Comprehensive Mechanical Properties of Pink Sheets Grade 319.0 T5 Alloy
- Pink Sheets 201.0 T7: High-Performance Mechanical Properties
- Pink Sheets Grade 201.0 T6: Comprehensive Mechanical Property Data
- Pink Sheets Grade 355.0 T71 – Comprehensive Mechanical Properties & Performance Data
- Pink Sheets Grade 319.0 T6 – Comprehensive Material Specifications
- Pink Sheets Grade 355.0 T51 – Comprehensive Material Specifications
- Pink Sheets Grade 356.0 T6: Premium Alloy for Superior Mechanical Strength
- Comprehensive Overview of Pink Sheets Grade 319.0 F – Properties & Standards
- Pink Sheets Grade 356.0 T7: Comprehensive Material Properties & Standards