Properties

General

PropertyValueCondition

Density

2.7 g/cm³

T6

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Compressive yield strength

172.0 - 186.0 MPa

T6

Elastic modulus

72.0 GPa

T6

72.4 GPa

T6

Elongation

-195 °C

3.5 %

T6

Sand cast, elongation in 50 mm

-80 °C

3.5 %

T6

Sand cast, elongation in 50 mm

-28 °C

3.5 %

T6

Sand cast, elongation in 50 mm

3.0 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

A100

3.8 %

T6

24 °C

3.5 %

T6

Sand cast, elongation in 50 mm

100 °C

4 %

T6

Sand cast, elongation in 50 mm

150 °C

6 %

T6

Sand cast, elongation in 50 mm

205 °C

18 %

T6

Sand cast, elongation in 50 mm

260 °C

35 %

T6

Sand cast, elongation in 50 mm

315 °C

60 %

T6

Sand cast, elongation in 50 mm

371 °C

80 %

T6

Sand cast, elongation in 50 mm

Fatigue strength

90 MPa

T6

for 5x10⁸ cycles, R.R. Moore type test

Hardness, Brinell

70.0 [-]

T6

Pink Sheets, ASTM B26, ASTM B618

Casting

80 [-]

T6

500 kg load, 10 mm b

85.0 [-]

T6

Pink Sheets, ASTM B108, ASTM B955

Casting

Poisson's ratio

0.33 [-]

T6

Shear modulus

27.2 GPa

T6

Shear strength

179 MPa

T6

Tensile strength

-195 °C

275 MPa

T6

Sand cast

-80 °C

240 MPa

T6

Sand cast

-28 °C

227 MPa

T6

Sand cast

205.0 MPa

T6

Pink Sheets, ASTM B26, ASTM B618

Casting

220.0 MPa

T6

230.0 MPa

T6

Pink Sheets, ASTM B108, ASTM B955

Casting

24 °C

227 MPa

T6

Sand cast

100 °C

220 MPa

T6

Sand cast

150 °C

160 MPa

T6

Sand cast

205 °C

83 MPa

T6

Sand cast

260 °C

53 MPa

T6

Sand cast

315 °C

28 MPa

T6

Sand cast

371 °C

17 MPa

T6

Sand cast

Yield strength

-195 °C

193 MPa

T6

Sand cast, RP02

-80 °C

172 MPa

T6

Sand cast, RP02

-28 °C

165 MPa

T6

Sand cast, RP02

140.0 MPa

T6

Pink Sheets, ASTM B26, ASTM B618

Casting

RP02

150.0 MPa

T6

Pink Sheets, ASTM B108, ASTM B955

Casting

RP02

170.0 MPa

T6

24 °C

165 MPa

T6

Sand cast, RP02

100 °C

165 MPa

T6

Sand cast, RP02

150 °C

138 MPa

T6

Sand cast, RP02

205 °C

58 MPa

T6

Sand cast, RP02

260 °C

35 MPa

T6

Sand cast, RP02

315 °C

21 MPa

T6

Sand cast, RP02

371 °C

14 MPa

T6

Sand cast, RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

2.2e-05 1/K

T6

Melting point

557.0 - 613.0 °C

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

570.0 °C

T6

Specific heat capacity

970.0 J/(kg·K)

T6

100 °C

960 J/(kg·K)

T6

derived value

Thermal conductivity

150.0 W/(m·K)

T6

25 °C

150 W/(m·K)

T6

derived value

Electrical

PropertyValueConditionComment

Electrical conductivity

23000000 S/m

T6

Typical/Derived values

Electrical resistivity

4.42e-08 Ω·m

T6

Typical values

Specific Electrical conductivity

39.0 - 41.0 % IACS

T6

Typical values

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

90.1 - 93.3 %

T6

Copper

0.25 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

Iron

0.6 %

T6

0.60 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

Magnesium

0.2 - 0.45 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

Manganese

0.35 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

Other

0.15 %

T6

Silicon

6.5 - 7.5 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

Titanium

0.25 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting

Zinc

0.35 %

T6

Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955

Casting


Metal

  1. Pink Sheets Grade 242.0 O – Comprehensive Material Properties & Standards
  2. Comprehensive Mechanical Properties of Pink Sheets Grade 319.0 T5 Alloy
  3. Pink Sheets 201.0 T7: High-Performance Mechanical Properties
  4. T61 Pink Sheets Grade 242.0 – Detailed Mechanical Properties
  5. Pink Sheets Grade 201.0 T6: Comprehensive Mechanical Property Data
  6. Pink Sheets Grade 319.0 T6 – Comprehensive Material Specifications
  7. T51 Pink Sheets Alloy – Grade 356.0 – Key Mechanical Properties
  8. Pink Sheets Grade 355.0 T6: Comprehensive Mechanical Properties & Standards
  9. Comprehensive Overview of Pink Sheets Grade 319.0 F – Properties & Standards
  10. Pink Sheets Grade 356.0 T7: Comprehensive Material Properties & Standards