Pink Sheets Grade 355.0 T51 – Comprehensive Material Specifications
Properties
General
| Property | Value | Condition |
|---|---|---|
Density | 2.8 g/cm³ | T51 |
Mechanical
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Compressive yield strength | 165 MPa | T51 | ||||
Elastic modulus | 76.0 GPa | T51 | ||||
25 °C | 70.3 GPa | T51 | ||||
150 °C | 67.6 GPa | T51 | ||||
204 °C | 64.1 GPa | T51 | ||||
260 °C | 56.5 GPa | T51 | ||||
Elongation | -195 °C | 1.5 % | T51 | Sand cast, elongation in 50 mm | ||
-80 °C | 1.5 % | T51 | Sand cast, elongation in 50 mm | |||
-28 °C | 1.5 % | T51 | Sand cast, elongation in 50 mm | |||
1.5 % | T51 | |||||
24 °C | 1.5 % | T51 | Sand cast, elongation in 50 mm | |||
100 °C | 2 % | T51 | Sand cast, elongation in 50 mm | |||
150 °C | 3 % | T51 | Sand cast, elongation in 50 mm | |||
205 °C | 8 % | T51 | Sand cast, elongation in 50 mm | |||
260 °C | 16 % | T51 | Sand cast, elongation in 50 mm | |||
315 °C | 36 % | T51 | Sand cast, elongation in 50 mm | |||
371 °C | 50 % | T51 | Sand cast, elongation in 50 mm | |||
Fatigue strength | 55 MPa | T51 | for 5x10⁸ cycles, R.R. Moore type test | |||
Hardness, Brinell | 65.0 - 90.0 [-] | T51 | 500 kg load, 10 mm b | |||
65.0 [-] | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
75.0 [-] | T51 | Pink Sheets, ASTM B108 | Casting | |||
Poisson's ratio | 0.33 [-] | T51 | ||||
Shear modulus | 26.2 GPa | T51 | ||||
Shear strength | 152 MPa | T51 | ||||
Tensile strength | -195 °C | 227 MPa | T51 | Sand cast | ||
-80 °C | 200 MPa | T51 | Sand cast | |||
-28 °C | 193 MPa | T51 | Sand cast | |||
170.0 MPa | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
185.0 MPa | T51 | Pink Sheets, ASTM B108 | Casting | |||
24 °C | 193 MPa | T51 | Sand cast | |||
100 °C | 193 MPa | T51 | Sand cast | |||
150 °C | 165 MPa | T51 | Sand cast | |||
205 °C | 95 MPa | T51 | Sand cast | |||
260 °C | 67 MPa | T51 | Sand cast | |||
315 °C | 40 MPa | T51 | Sand cast | |||
371 °C | 25 MPa | T51 | Sand cast | |||
Yield strength | -195 °C | 185 MPa | T51 | Sand cast, RP02 | ||
-80 °C | 165 MPa | T51 | Sand cast, RP02 | |||
-28 °C | 160 MPa | T51 | Sand cast, RP02 | |||
125.0 MPa | T51 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 | ||
150.0 MPa | T51 | |||||
24 °C | 160 MPa | T51 | Sand cast, RP02 | |||
100 °C | 152 MPa | T51 | Sand cast, RP02 | |||
150 °C | 130 MPa | T51 | Sand cast, RP02 | |||
205 °C | 70 MPa | T51 | Sand cast, RP02 | |||
260 °C | 35 MPa | T51 | Sand cast, RP02 | |||
315 °C | 21 MPa | T51 | Sand cast, RP02 | |||
371 °C | 14 MPa | T51 | Sand cast, RP02 |
Thermal
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2.3e-05 1/K | T51 | ||||
100 °C | 0.0000223 1/K | T51 | nominal value between 20°C and the mentioned temperature | |||
300 °C | 0.0000247 1/K | T51 | nominal value between 20°C and the mentioned temperature | |||
Melting point | 546.0 - 621.0 °C | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting | ||
560.0 °C | T51 | |||||
Specific heat capacity | 880.0 J/(kg·K) | T51 | ||||
Thermal conductivity | 170.0 W/(m·K) | T51 | ||||
25 °C | 167 W/(m·K) | T51 | unstated value |
Electrical
| Property | Value | Condition | Comment |
|---|---|---|---|
Electrical conductivity | 24939999.999999996 S/m | T51 | Typical/Derived values |
Electrical resistivity | 4.0099999999999995e-08 Ω·m | T51 | Typical values |
Specific Electrical conductivity | 43 % IACS | T51 | Typical values |
Chemical properties
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Aluminium | 90.3 - 94.1 % | T51 | ||
Chromium | 0.25 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Copper | 1.0 - 1.5 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Iron | 0.6 % | T51 | ||
0.60 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting | |
Magnesium | 0.4 - 0.6 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Manganese | 0.5 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Other | 0.15 % | T51 | ||
Silicon | 4.5 - 5.5 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Titanium | 0.25 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Zinc | 0.35 % | T51 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Metal
- Pink Sheets Grade 242.0 O – Comprehensive Material Properties & Standards
- Comprehensive Mechanical Properties of Pink Sheets Grade 319.0 T5 Alloy
- Pink Sheets 201.0 T7: High-Performance Mechanical Properties
- T61 Pink Sheets Grade 242.0 – Detailed Mechanical Properties
- Pink Sheets Grade 201.0 T6: Comprehensive Mechanical Property Data
- Pink Sheets Grade 355.0 T71 – Comprehensive Mechanical Properties & Performance Data
- Pink Sheets Grade 319.0 T6 – Comprehensive Material Specifications
- T51 Pink Sheets Alloy – Grade 356.0 – Key Mechanical Properties
- Pink Sheets Grade 355.0 T6: Comprehensive Mechanical Properties & Standards
- Comprehensive Overview of Pink Sheets Grade 319.0 F – Properties & Standards