VdTÜV WB 230-3 Annealed TiNi0.8Mo0.3 Alloy – Premium Corrosion‑Resistant Titanium Grade
This DIN TiNi0.8Mo0.3 alloy is similar to Titanium Grades 2 and 3 except that DIN TiNi0.8Mo0.3 has 0.3% molybdenum and 0.8% nickel. This alloy also offers enhanced corrosion resistance.
Properties
General
| Property | Temperature | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|---|
Density | 20.0 °C | 4.505 g/cm³ | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Flat |
20.0 °C | 4.51 g/cm³ | Annealed | DIN 17851, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-3 | Forging, Rod, Welded Tube |
Mechanical
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 103.0 GPa | Annealed | DIN 17851, DIN 17864, DIN 17862, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3 | Forging, Rod, Welded Tube | |
20.0 °C | 108.0 - 110.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar | ||
200.0 °C | 96.0 - 97.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar | ||
400.0 °C | 82.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar | ||
Elongation | 20.0 °C | 16.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod | Transverse |
20.0 °C | 18.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Welded Tube | ||
Hardness, Brinell | 20.0 °C | 170.0 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod | |
20.0 °C | 170.0 | Annealed | DIN 17864, DIN 17851, DIN 17862, DIN 17860 | Forging | Transverse | |
Reduction of area | 20.0 °C | 25.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod | |
Tensile strength | 20.0 °C | 480.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Welded Tube | |
20.0 °C | 480.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod | Transverse | |
20.0 °C | 560.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | |||
100.0 °C | 460.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | |||
200.0 °C | 340.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 | |||
300.0 °C | 260.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2 |
Thermal
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Coefficient of thermal expansion | 7.599999999999997e-06 - 1.1e-05 1/K | Typical for Titanium Near Alpha Alloy | ||||
Melting point | 1540.0 - 1715.0 °C | Typical for Titanium Near Alpha Alloy | ||||
Specific heat capacity | 20.0 °C | 520.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Flat | |
200.0 °C | 570.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Flat | ||
400.0 °C | 630.0 J/(kg·K) | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Flat | ||
Thermal conductivity | 20.0 °C | 19.0 W/(m·K) | Annealed | DIN 17851, DIN 17864, DIN 17862, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3 | Forging, Rod, Welded Tube | |
20.0 °C | 22.6 W/(m·K) | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar | ||
200.0 °C | 20.9 W/(m·K) | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar | ||
400.0 °C | 19.3 W/(m·K) | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar |
Electrical
| Property | Temperature | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|---|
Electrical resistivity | 20.0 °C | 5.2e-07 Ω·m | Annealed | DIN 17851, DIN 17864, DIN 17862, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17850 | Forging, Rod, Welded Tube, Tube, Flat, Wire, Bar |
200.0 °C | 8.7e-07 Ω·m | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar | |
400.0 °C | 1.2e-06 Ω·m | Annealed | DIN 17851, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Tube, Flat, Wire, Bar |
Chemical properties
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Carbon | 0.06 | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Welded Tube, Flat |
Hydrogen | 0.013 | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Welded Tube, Flat |
Iron | 0.25 | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Welded Tube, Flat |
Molybdenum | 0.2 - 0.4 % | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Welded Tube, Flat |
Nickel | 0.6 - 0.9 % | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Welded Tube, Flat |
Nitrogen | 0.03 | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Welded Tube, Flat |
Oxygen | 0.25 | Annealed | VdTÜV WB 230-3, DIN 17851, DIN 17862, DIN 17864, DIN 17860, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2 | Forging, Rod, Wire, Bar, Tube, Welded Tube, Flat |
Titanium | 97.7 % | Annealed | DIN 17851, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-3 | Tube, Forging, Rod, Welded Tube |
Metal
- VdTÜV WB 230-3: Premium Ti1 Titanium Grade for Advanced Welding Applications
- High-Performance Ti2 Titanium Grade for Welding Applications
- VdTÜV WB 230-3 Ti3 Grade Titanium – High-Strength, Welded Form
- VdTÜV Certified WB 230-3 Grade Ti4 Titanium Welded Alloy – Premium Strength & Corrosion Resistance
- DIN 17850 Grade Ti3Pd Annealed Titanium – Low‑Alloy, High‑Performance for Pressure & Nuclear Applications
- DIN Ti1 Titanium – High Ductility, Superior Corrosion Resistance, Ideal for Precision Applications
- VdTÜV WB 230-3 Ti3 Titanium – Annealed, High Strength & Corrosion Resistant
- Premium VdTÜV WB 230-3 Grade Ti4 – Annealed Titanium for Superior Strength
- DIN 17850 Ti1Pd Annealed: Premium Corrosion‑Resistant Titanium Alloy
- VdTÜV WB 230-3 Ti2 Titanium – Annealed Grade with Superior Strength and Welding