DIN 17850 Grade Ti3Pd Annealed Titanium – Low‑Alloy, High‑Performance for Pressure & Nuclear Applications
Low-alloy titanium for seamless pipes for pressure equipment requiring monitoring acc. to AD 2000 W0, directive 2014/68/EU and for nuclear engineering.
Properties
General
| Property | Temperature | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|---|
Density | 20.0 °C | 4.505 g/cm³ | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Mechanical
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Elastic modulus | 20.0 °C | 108.0 - 110.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube | |
20.0 °C | 108.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
200.0 °C | 96.0 - 97.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube | ||
200.0 °C | 96.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
400.0 °C | 82.0 GPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
Elongation | 20.0 °C | 16.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 17.0 % | Annealed | DIN 17851, DIN 17864, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17860 | Welded Tube | ||
20.0 °C | 18.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Hardness, Brinell | 20.0 °C | 170.0 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | |
Reduction of area | 20.0 °C | 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse |
20.0 °C | 30.0 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | ||
Shear modulus | 20.0 °C | 45.0 GPa | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | |
Tensile strength | 20.0 °C | 460.0 - 590.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Welded Tube | |
20.0 °C | 460.0 - 590.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod | Transverse | |
20.0 °C | 560.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
100.0 °C | 460.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
200.0 °C | 340.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | |||
300.0 °C | 260.0 MPa | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 |
Thermal
| Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
|---|---|---|---|---|---|---|
Coefficient of thermal expansion | 200.0 °C | 9.1e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | |
400.0 °C | 9.2e-06 1/K | Annealed | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Welded Tube | ||
Melting point | 1540.0 - 1715.0 °C | Typical for Titanium Near Alpha Alloy | ||||
Specific heat capacity | 20.0 °C | 520.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
200.0 °C | 570.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
400.0 °C | 630.0 J/(kg·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
Thermal conductivity | 20.0 °C | 22.6 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
200.0 °C | 20.9 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | ||
400.0 °C | 19.3 W/(m·K) | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Electrical
| Property | Temperature | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|---|
Electrical resistivity | 20.0 °C | 5.2e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
200.0 °C | 8.7e-07 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube | |
400.0 °C | 1.2e-06 Ω·m | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Chemical properties
| Property | Value | Condition | Related Standards | Shape |
|---|---|---|---|---|
Carbon | 0.06 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Hydrogen | 0.013 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Iron | 0.25 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Nitrogen | 0.05 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Oxygen | 0.25 | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Palladium | 0.15 - 0.25 % | Annealed | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Forging, Rod, Tube, Welded Tube |
Titanium | 98.7 % | Annealed | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tube, Forging, Rod, Welded Tube |
Metal
- DIN 17442 X38CrMoV15 Soft-Annealed Stainless Steel – Superior Corrosion Resistance
- DIN 17210 Grade 21NiCrMo2 Soft Annealed Steel – Superior Wear Resistance & Fatigue Strength
- DIN 17850 Grade Ti3 ½ Hard Titanium – High Strength & Corrosion Resistance
- DIN 2391-2 St 30 Al Seamless Steel Tube – Soft Annealed, Grade A
- DIN 2391-2 St 30 Si Soft‑Annealed Tube – Grade A for Precision Construction
- VdTÜV WB 230-3 Annealed TiNi0.8Mo0.3 Alloy – Premium Corrosion‑Resistant Titanium Grade
- DIN 17851 TiAl6V6Sn2 Annealed Alloy: Superior Strength & Corrosion Resistance for Aerospace
- DIN Ti1 Titanium – Softest Grade with Superior Ductility, Corrosion & Welding Performance
- DIN 17850 Ti1Pd Annealed: Premium Corrosion‑Resistant Titanium Alloy
- DIN 17850 Ti2Pd: Premium Grade Titanium Alloy (Annealed)