Industrial manufacturing
Industrial Internet of Things | Industrial materials | Equipment Maintenance and Repair | Industrial programming |
home  MfgRobots >> Industrial manufacturing >  >> Industrial materials >> Metal

VdTÜV WB 230-3 Ti2 Titanium – Annealed Grade with Superior Strength and Welding

DIN Ti2 titanium is the second of four commercially unalloyed titanium grades. It has a moderate strength as well as excellent welding properties. The material is known for its good resistance to oxidation and corrosion.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20.0 °C

4.505 g/cm³

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

20.0 °C

110.0 GPa

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

200.0 °C

97.0 GPa

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

400.0 °C

82.0 GPa

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

Elongation

20.0 °C

20.0 %

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Forging

Transverse

20.0 °C

20.0 %

Annealed

WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Forging, Rod

20.0 °C

22.0 %

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Welded Tube, Wire, Sheet

Hardness, Brinell

20.0 °C

150.0

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Forging, Rod

20.0 °C

150.0

Annealed

DIN 17864, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17860

Forging

Transverse

Poisson's ratio

0.361 [-]

Typical for Pure Titanium

Reduction of area

20.0 °C

30.0 %

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Forging

Transverse

20.0 °C

30.0 %

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Forging, Rod

Shear modulus

20.0 °C

45.0 GPa

Annealed

WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Sheet

Tensile strength

20.0 °C

390.0 - 540.0 MPa

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Welded Tube, Wire, Sheet

20.0 °C

390.0 - 540.0 MPa

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Forging

Transverse

20.0 °C

470.0 MPa

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

100.0 °C

370.0 MPa

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

200.0 °C

260.0 MPa

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

300.0 °C

190.0 MPa

Annealed

DIN 17850, VdTÜV WB 230-3, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

8.400000000000001e-06 - 8.599999999999999e-06 1/K

Typical for Pure Titanium

Melting point

1670.0 °C

Typical for Pure Titanium

Specific heat capacity

20.0 °C

520.0 J/(kg·K)

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

200.0 °C

570.0 J/(kg·K)

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

400.0 °C

630.0 J/(kg·K)

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

Thermal conductivity

20.0 °C

22.6 W/(m·K)

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

200.0 °C

20.9 W/(m·K)

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

400.0 °C

19.3 W/(m·K)

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical resistivity

20.0 °C

4.8e-07 Ω·m

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

200.0 °C

8e-07 Ω·m

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

400.0 °C

1.14e-06 Ω·m

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

Chemical properties

PropertyValueConditionRelated StandardsShape

Carbon

0.06

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat

0.08

Annealed

WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Sheet

Hydrogen

0.013

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat, Sheet

Iron

0.2

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat

0.25

Annealed

WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Sheet

Nitrogen

0.05

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat

0.06

Annealed

WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Sheet

Oxygen

0.18

Annealed

VdTÜV WB 230-3, WL 3.7034-1, DIN 17850, DIN 17862, DIN 17864, DIN 17860, VdTÜV WB 230-1, VdTÜV WB 230-2

Forging, Rod, Wire, Tube, Welded Tube, Flat

0.25

Annealed

WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Sheet

Titanium

98.7 %

Annealed

WL 3.7034-1, DIN 17850, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Forging, Rod, Sheet

99.1 %

Annealed

DIN 17850, VdTÜV WB 230-2, WL 3.7034-1, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860

Tube, Forging, Rod, Welded Tube, Wire, Flat


Metal

  1. VdTÜV WB 230-3: Premium Ti1 Titanium Grade for Advanced Welding Applications
  2. High-Performance Ti2 Titanium Grade for Welding Applications
  3. VdTÜV WB 230-3 Annealed TiNi0.8Mo0.3 Alloy – Premium Corrosion‑Resistant Titanium Grade
  4. DIN 17850 Grade Ti3Pd Annealed Titanium – Low‑Alloy, High‑Performance for Pressure & Nuclear Applications
  5. DIN Ti1 Titanium – High Ductility, Superior Corrosion Resistance, Ideal for Precision Applications
  6. VdTÜV WB 230-3 Ti3 Titanium – Annealed, High Strength & Corrosion Resistant
  7. Premium VdTÜV WB 230-3 Grade Ti4 – Annealed Titanium for Superior Strength
  8. DIN 17850 Ti1Pd Annealed: Premium Corrosion‑Resistant Titanium Alloy
  9. DIN 17850 Ti2Pd: Premium Grade Titanium Alloy (Annealed)
  10. VdTÜV WB 230-3 Ti2 Titanium – Annealed Grade with Superior Strength and Welding