Industrial manufacturing
Industrial Internet of Things | Industrial materials | Equipment Maintenance and Repair | Industrial programming |
home  MfgRobots >> Industrial manufacturing >  >> Industrial materials >> Metal

SEW 385 Grade Ni46 Soft‑Annealed Alloy (+A) – High‑Performance Thermal Expansion Solution

The iron alloy with special thermal expansion Ni46, material number 1.3920, is used for compounds of metal and glass and for compounds of metal and ceramics, for expansion governors as well as for bimetals (according to DIN 1715). The break point temperature (temperature at which a break point in the expansion-temperature-curve occurs) is 400 degrees C. The cupping index at 1 mm thickness is 10.5 mm.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8.2 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

152 GPa

Elongation

20.0 °C

30 %

Poisson's ratio

23.0 °C

0.29 [-]

Typical for Nickel Steel

Shear modulus

23.0 °C

76 GPa

Typical for Nickel Steel

Tensile strength

20.0 °C

440 - 640 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

7.9E-6 1/K

150.0 °C

7.8E-6 1/K

200.0 °C

7.7E-6 1/K

300.0 °C

7.4E-6 1/K

400.0 °C

7.3E-6 1/K

500.0 °C

8.6E-6 1/K

600.0 °C

9.7E-6 1/K

Melting point

1316 - 1595 °C

Typical for Nickel Steel

Specific heat capacity

23.0 °C

456 J/(kg·K)

Typical for Nickel Steel

Thermal conductivity

20.0 °C

15 - 17 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

5.5E-7 - 6E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.05 - 0.1 %

Manganese

1 %

Nickel

45 - 47 %

Silicon

0.3 - 0.5 %


Metal

  1. SEW 385 Grade Ni36 Soft Annealed (+A) – Ultra‑Low Expansion Alloy for Optics, Antennas & Measurement Tech
  2. SEW 385 Ni42 Soft-Annealed Alloy (+A) – Low-Expansion, High-Performance Material
  3. SEW 400 X105CrMo17 Soft-Annealed Steel (+A): Superior Hardening and Wear Resistance
  4. SEW 400 X65Cr13 Stainless Steel – Soft Annealed, Superior Cutting Tool Performance
  5. SEW 400 X55CrMo14 Soft Annealed Steel – High-Performance Cutting & Bearing Applications
  6. SEW 400 X90CrMoV18 Soft-Annealed Steel: Superior Corrosion & Wear Resistance
  7. SEW 400 X2Cr11 Soft-Annealed Stainless Steel – Superior Corrosion Resistance & Strength
  8. SEW 400 Grade X1CrTi15 Soft Annealed Stainless Steel (+A) – High Performance Low‑Carbon Alloy for Automotive & Industrial Use
  9. SEW 400 X2CrMoNb18-2 Steel – Soft-Annealed Grade (+A) for High-Performance Applications
  10. SEW 470 Grade X3CrAlTi18-2 Soft Annealed Steel (+A): 1000 °C Resistance