X12Cr13 Soft Annealed Steel (EN 10250-4): Key Properties & Industrial Uses
The make X12Cr13 is comparable to X 10 Cr 13 acc. to DIN 17440 : 1985-07. The material is applicated for construction parts in water and steam and mild acting media of food industry, predominantly in tempered condition (fitting parts, valve spindles, shafts, pump components, bolts, screws) with honed or polished surface.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.7 - 7.73 g/cm³ |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | 20.0 °C | 215 - 217.99 GPa |
100.0 °C | 212 - 215 GPa | |
200.0 °C | 188 - 205.94 GPa | |
300.0 °C | 164 - 200 GPa | |
400.0 °C | 188.79 - 190 GPa | |
Hardness, Brinell | 20.0 °C | 220 [-] |
Poisson's ratio | 20.0 °C | 0.29 [-] |
100.0 °C | 0.29 [-] | |
200.0 °C | 0.29 [-] | |
300.0 °C | 0.31 [-] | |
400.0 °C | 0.31 [-] | |
Shear modulus | 20.0 °C | 84.82 GPa |
100.0 °C | 82.5 GPa | |
200.0 °C | 79.57 GPa | |
300.0 °C | 75.86 GPa | |
400.0 °C | 72 GPa | |
Tensile strength | 20.0 °C | 730 MPa |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | 20.0 °C | 1.02E-5 1/K | |
100.0 °C | 1.05E-5 1/K | ||
200.0 °C | 1.09E-5 - 1.1E-5 1/K | ||
300.0 °C | 1.13E-5 - 1.15E-5 1/K | ||
400.0 °C | 1.16E-5 - 1.2E-5 1/K | ||
500.0 °C | 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K | ||
Melting point | 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Specific heat capacity | 20.0 °C | 439 - 460 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) | ||
200.0 °C | 498 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 25.9 - 30 W/(m·K) | |
100.0 °C | 25.3 W/(m·K) | ||
200.0 °C | 25.2 W/(m·K) | ||
300.0 °C | 25.2 W/(m·K) | ||
400.0 °C | 25.4 W/(m·K) | ||
500.0 °C | 25.7 W/(m·K) | ||
600.0 °C | 25.9 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 7.6 mm²/s | |
100.0 °C | 6.6 mm²/s | ||
200.0 °C | 6.1 mm²/s | ||
300.0 °C | 5.8 mm²/s | ||
400.0 °C | 5.3 mm²/s | ||
500.0 °C | 4.8 mm²/s | ||
600.0 °C | 4.1 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 5.59E-7 Ω·m |
100.0 °C | 6.4E-7 Ω·m | |
200.0 °C | 7.32E-7 Ω·m | |
300.0 °C | 8.17E-7 Ω·m | |
400.0 °C | 8.97E-7 Ω·m | |
500.0 °C | 9.74E-7 Ω·m | |
600.0 °C | 1.05E-6 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.08 - 0.15 % |
Chromium | 11.5 - 13.5 % |
Manganese | 1.5 % |
Nickel | 0.75 % |
Phosphorus | 0.04 % |
Silicon | 1 % |
Sulfur | 0.03 % |
Metal
- EN 10088-1 X70CrMo15: Soft Annealed Grade for Cutting Tools & Industrial Applications
- Premium Soft-Annealed X12Cr13 Steel – EN 10272 for Pressure Vessels
- EN 10250-4 Grade X17CrNi16-2 Soft-Annealed Steel (+A) – Premium Corrosion Resistance & Wear Performance
- EN 10250‑4 Grade X20Cr13 Soft Annealed Steel – High Strength, Corrosion‑Resistant Performance
- EN 10250-4 Grade X30Cr13 Soft Annealed: Premium Corrosion-Resistant Alloy for Precision Applications
- EN 10250‑4 Grade X3CrNiMo13‑4 Soft‑Annealed (+A) – Premium Corrosion‑Resistant Steel
- EN 10250-4 Grade X4CrNiMo16-5-1 Soft Annealed Stainless Steel (+A) – High Corrosion Resistance & Low‑Temperature Performance
- EN 10250-4 X6CrAl13 Soft Annealed (+A) – Superior Alloy for Petroleum & Power Plant Applications
- EN 10250-4 Grade X6Cr17 – Soft Annealed Ferritic Steel for Corrosion Resistance
- DIN 17440 Grade X12Cr13 Soft Annealed (+A) – Premium Stainless Steel for Pressure Vessels & Food Industry