EN 10132-4 Grade Ck75 – Cold Rolled, Quenched & Tempered Steel
The steel Ck 75 is used as cold rolled steel strip for springs with high dimensional accuracy and surface condition up to 2.0 mm thicknesses.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.8 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 206 - 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Hardness, Vickers | 20.0 °C | 390 - 555 [-] | |
Poisson's ratio | 20.0 °C | 0.29 [-] | Typical for High Carbon Steel |
Shear modulus | 20.0 °C | 78 GPa | |
Tensile strength | 20.0 °C | 1320 - 1870 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K | ||
Melting point | 1289 - 1478 °C | Typical for High Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41.7 W/(m·K) | |
100.0 °C | 43.4 W/(m·K) | ||
200.0 °C | 43.2 W/(m·K) | ||
300.0 °C | 41.4 W/(m·K) | ||
400.0 °C | 39.1 W/(m·K) | ||
500.0 °C | 36.7 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.6 mm²/s | |
100.0 °C | 11.3 mm²/s | ||
200.0 °C | 10.5 mm²/s | ||
300.0 °C | 9.5 mm²/s | ||
400.0 °C | 8.3 mm²/s | ||
500.0 °C | 7.1 mm²/s | ||
600.0 °C | 5.8 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.5E-7 Ω·m |
100.0 °C | 2.95E-7 Ω·m | |
200.0 °C | 3.65E-7 Ω·m | |
300.0 °C | 4.53E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m | |
500.0 °C | 6.74E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.7 - 0.8 % |
Manganese | 0.6 - 0.8 % |
Phosphorus | 0.04 % |
Silicon | 0.15 - 0.35 % |
Sulfur | 0.035 % |
Metal
- EN 10132-4 Grade 71Si7 Cold Rolled, Quenched & Tempered Steel – Ideal for High-Load Tension Springs
- EN 10132-4 Grade 50CrV4 Cold Rolled, Quenched & Tempered Steel – High Precision Spring Strip
- EN 10132-4 Grade Ck85: Cold Rolled, Quenched & Tempered Steel for Precision Springs
- EN 10132-4 Grade 67SiCr5 – Cold Rolled, Quenched & Tempered Steel for High‑Precision Springs
- EN 10277-3 Grade 46SPb20: Premium Cold‑Drawn, Quenched & Tempered Steel for High‑Strength Applications
- EN 10277-5 Grade 42CrMoS4 – Premium Cold‑Drawn, Quenched & Tempered Steel for High‑Load Automotive & Machinery
- EN 10277‑3 Grade 35SPb20 – Cold‑Drawn, Quenched & Tempered Steel for High‑Strength Applications
- EN 10277-5 Grade 34CrS4 Cold-Drawn, Quenched & Tempered Steel – Premium Performance for Automotive & Machinery
- 41CrS4 Cold‑Drawn, Quenched & Tempered Steel – EN 10277‑5 Specification for Automotive & Machine Components
- EN 10277‑5 Grade 51CrV4 Cold‑Drawn, Quenched & Tempered Steel (+C+QT) – High‑Performance Alloy for Aerospace & Heavy Machinery