EN 10132-4 Grade Ck85: Cold Rolled, Quenched & Tempered Steel for Precision Springs
The steel Ck 85 is used as cold rolled steel strip for springs with high dimensional accuracy and surface condition up to 2.5 mm thicknesses.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.8 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa | |
20.0 °C | 206 - 212 GPa | ||
100.0 °C | 207 GPa | ||
200.0 °C | 199 GPa | ||
300.0 °C | 192 GPa | ||
400.0 °C | 184 GPa | ||
500.0 °C | 175 GPa | ||
600.0 °C | 164 GPa | ||
Hardness, Vickers | 20.0 °C | 415 - 580 [-] | |
Poisson's ratio | 20.0 °C | 0.29 [-] | Typical for High Carbon Steel |
Shear modulus | 20.0 °C | 78 GPa | |
Tensile strength | 20.0 °C | 1400 - 1950 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K | ||
Melting point | 1289 - 1478 °C | Typical for High Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41.7 W/(m·K) | |
100.0 °C | 43.4 W/(m·K) | ||
200.0 °C | 43.2 W/(m·K) | ||
300.0 °C | 41.4 W/(m·K) | ||
400.0 °C | 39.1 W/(m·K) | ||
500.0 °C | 36.7 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.6 mm²/s | |
100.0 °C | 11.3 mm²/s | ||
200.0 °C | 10.5 mm²/s | ||
300.0 °C | 9.5 mm²/s | ||
400.0 °C | 8.3 mm²/s | ||
500.0 °C | 7.1 mm²/s | ||
600.0 °C | 5.8 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.5E-7 Ω·m |
100.0 °C | 2.95E-7 Ω·m | |
200.0 °C | 3.65E-7 Ω·m | |
300.0 °C | 4.53E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m | |
500.0 °C | 6.74E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.8 - 0.9 % |
Manganese | 0.45 - 0.65 % |
Phosphorus | 0.04 % |
Silicon | 0.15 - 0.35 % |
Sulfur | 0.035 % |
Metal
- EN 10132-4 Grade 71Si7 Cold Rolled, Quenched & Tempered Steel – Ideal for High-Load Tension Springs
- EN 10132-4 Grade 50CrV4 Cold Rolled, Quenched & Tempered Steel – High Precision Spring Strip
- EN 10132-4 Grade Ck75 – Cold Rolled, Quenched & Tempered Steel
- EN 10132-4 Grade Ck85: Cold Rolled, Quenched & Tempered Steel for Precision Springs
- EN 10132-4 Grade 67SiCr5 – Cold Rolled, Quenched & Tempered Steel for High‑Precision Springs
- EN 10277-3 Grade 46SPb20: Premium Cold‑Drawn, Quenched & Tempered Steel for High‑Strength Applications
- EN 10277-5 Grade 42CrMoS4 – Premium Cold‑Drawn, Quenched & Tempered Steel for High‑Load Automotive & Machinery
- EN 10277‑3 Grade 35SPb20 – Cold‑Drawn, Quenched & Tempered Steel for High‑Strength Applications
- EN 10277-5 Grade 34CrS4 Cold-Drawn, Quenched & Tempered Steel – Premium Performance for Automotive & Machinery
- 41CrS4 Cold‑Drawn, Quenched & Tempered Steel – EN 10277‑5 Specification for Automotive & Machine Components