EN 10132-4 Grade 67SiCr5 – Cold Rolled, Quenched & Tempered Steel for High‑Precision Springs
The steel 67 SiCr 5 is used as cold rolled steel strip for springs with high dimensional accuracy and surface condition up to 3.0 mm thicknesses.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.83 g/cm³ |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | -100.0 °C | 217 GPa |
20.0 °C | 206 - 212 GPa | |
100.0 °C | 207 GPa | |
200.0 °C | 199 GPa | |
300.0 °C | 192 GPa | |
400.0 °C | 184 GPa | |
500.0 °C | 175 GPa | |
600.0 °C | 164 GPa | |
Hardness, Vickers | 20.0 °C | 445 - 650 [-] |
Poisson's ratio | 20.0 °C | 0.28 [-] |
Shear modulus | 20.0 °C | 78 GPa |
Tensile strength | 20.0 °C | 1500 - 2200 MPa |
Thermal
| Property | Temperature | Value |
|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K |
20.0 °C | 1.15E-5 1/K | |
100.0 °C | 1.21E-5 1/K | |
200.0 °C | 1.27E-5 1/K | |
300.0 °C | 1.32E-5 1/K | |
400.0 °C | 1.36E-5 1/K | |
500.0 °C | 1.4E-5 1/K | |
600.0 °C | 1.44E-5 1/K | |
Max service temperature, long | 0 - 300 °C | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) |
20.0 °C | 461 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) | |
200.0 °C | 499 J/(kg·K) | |
300.0 °C | 517 J/(kg·K) | |
400.0 °C | 536 J/(kg·K) | |
500.0 °C | 558 J/(kg·K) | |
600.0 °C | 587 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 45.1 W/(m·K) |
100.0 °C | 45.1 W/(m·K) | |
200.0 °C | 44.1 W/(m·K) | |
300.0 °C | 41.9 W/(m·K) | |
400.0 °C | 39.4 W/(m·K) | |
500.0 °C | 36.9 W/(m·K) | |
600.0 °C | 34.4 W/(m·K) | |
Thermal diffusivity | 20.0 °C | 12.5 mm²/s |
100.0 °C | 11.6 mm²/s | |
200.0 °C | 10.6 mm²/s | |
300.0 °C | 9.5 mm²/s | |
400.0 °C | 8.4 mm²/s | |
500.0 °C | 7.1 mm²/s | |
600.0 °C | 5.8 mm²/s | |
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 2.31E-7 Ω·m |
100.0 °C | 2.84E-7 Ω·m | |
200.0 °C | 3.58E-7 Ω·m | |
300.0 °C | 4.48E-7 Ω·m | |
400.0 °C | 5.52E-7 Ω·m | |
500.0 °C | 6.71E-7 Ω·m | |
600.0 °C | 8.06E-7 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.62 - 0.72 % |
Chromium | 0.4 - 0.6 % |
Manganese | 0.4 - 0.6 % |
Phosphorus | 0.04 % |
Silicon | 1.2 - 1.4 % |
Sulfur | 0.035 % |
Metal
- EN 10132-4 Grade 71Si7 Cold Rolled, Quenched & Tempered Steel – Ideal for High-Load Tension Springs
- EN 10132-4 Grade 50CrV4 Cold Rolled, Quenched & Tempered Steel – High Precision Spring Strip
- EN 10132-4 Grade Ck75 – Cold Rolled, Quenched & Tempered Steel
- EN 10132-4 Grade Ck85: Cold Rolled, Quenched & Tempered Steel for Precision Springs
- EN 10277-3 Grade 46SPb20: Premium Cold‑Drawn, Quenched & Tempered Steel for High‑Strength Applications
- EN 10277-5 Grade 42CrMoS4 – Premium Cold‑Drawn, Quenched & Tempered Steel for High‑Load Automotive & Machinery
- EN 10277‑3 Grade 35SPb20 – Cold‑Drawn, Quenched & Tempered Steel for High‑Strength Applications
- EN 10277-5 Grade 34CrS4 Cold-Drawn, Quenched & Tempered Steel – Premium Performance for Automotive & Machinery
- 41CrS4 Cold‑Drawn, Quenched & Tempered Steel – EN 10277‑5 Specification for Automotive & Machine Components
- EN 10277‑5 Grade 51CrV4 Cold‑Drawn, Quenched & Tempered Steel (+C+QT) – High‑Performance Alloy for Aerospace & Heavy Machinery