EN 10216-2 Grade X11CrMo9-1+I Seamless Steel Tubes – Isothermally Annealed for High‑Temperature Pressure Applications
Seamless steel tube for pressure purposes with specified elevated temperature properties. The steel grade meet the essential requirements of Directive 97/23/EC.,Seamless tubes of the high-temperature X11CrMo9-1+I are used in steam boiler and pipeline construction, pressure vessel and apparatus engineering, especially in chemical industry and power station construction at temperatures from approx. 200 °C to maximum 400 °C and simultaneously high pressures. The total load and the special scaling circumstances can decrease or increase the temperature limit. Weldability is available.,Seamless tubes of the high-temperature X11CrMo9-1+I are used in steam boiler and pipeline construction, pressure vessel and apparatus engineering, especially in chemical industry and power station construction at temperatures up to approx. 550 °C and simultaneously high pressures. The total load and the special scaling circumstances can decrease or increase the temperature limit. When welding it should be considered that the behavior of the steel depends during and after welding on the applied heat treatment, the preparation and execution of the welding.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.77 g/cm³ |
Mechanical
| Property | Temperature | Value | Comment |
|---|---|---|---|
Elastic modulus | 20.0 °C | 218 GPa | |
100.0 °C | 213 GPa | ||
200.0 °C | 206 GPa | ||
300.0 °C | 198 GPa | ||
400.0 °C | 190 GPa | ||
500.0 °C | 180 GPa | ||
600.0 °C | 167 GPa | ||
700.0 °C | 150 GPa | ||
Elongation | 20.0 °C | 20 % | |
Elongation, transverse | 20.0 °C | 18 % | |
Poisson's ratio | 20.0 °C | 0.29 [-] | Typical for Chromium Molybdenum Steel |
Tensile strength | 20.0 °C | 460 - 640 MPa | |
Tensile strength, transverse | 20.0 °C | 460 - 640 MPa | |
Yield strength Rp0.2 | 20.0 °C | 210 MPa | |
100.0 °C | 187 MPa | ||
150.0 °C | 186 MPa | ||
200.0 °C | 178 MPa | ||
250.0 °C | 177 MPa | ||
300.0 °C | 175 MPa | ||
350.0 °C | 171 MPa | ||
400.0 °C | 164 MPa | ||
450.0 °C | 153 MPa | ||
500.0 °C | 142 MPa | ||
550.0 °C | 120 MPa | ||
Yield strength Rp0.2, transverse | 20.0 °C | 210 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1E-5 1/K | |
20.0 °C | 1.08E-5 1/K | ||
100.0 °C | 1.13E-5 1/K | ||
200.0 °C | 1.18E-5 1/K | ||
300.0 °C | 1.23E-5 1/K | ||
400.0 °C | 1.27E-5 1/K | ||
500.0 °C | 1.3E-5 1/K | ||
600.0 °C | 1.32E-5 1/K | ||
700.0 °C | 1.33E-5 1/K | ||
Max service temperature, long | 0 - 550 °C | ||
Melting point | 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | 20.0 °C | 429 J/(kg·K) | |
100.0 °C | 464 J/(kg·K) | ||
200.0 °C | 492 J/(kg·K) | ||
300.0 °C | 511 J/(kg·K) | ||
400.0 °C | 531 J/(kg·K) | ||
500.0 °C | 554 J/(kg·K) | ||
600.0 °C | 585 J/(kg·K) | ||
700.0 °C | 626 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 20.7 W/(m·K) | |
100.0 °C | 22.6 W/(m·K) | ||
200.0 °C | 24.4 W/(m·K) | ||
300.0 °C | 25.8 W/(m·K) | ||
400.0 °C | 26.9 W/(m·K) | ||
500.0 °C | 27.8 W/(m·K) | ||
600.0 °C | 28.5 W/(m·K) | ||
700.0 °C | 28.8 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 6.2 mm²/s | |
100.0 °C | 5.9 mm²/s | ||
200.0 °C | 6 mm²/s | ||
300.0 °C | 6 mm²/s | ||
400.0 °C | 5.7 mm²/s | ||
500.0 °C | 5.4 mm²/s | ||
600.0 °C | 4.8 mm²/s | ||
700.0 °C | 4 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 5.03E-7 Ω·m |
100.0 °C | 5.67E-7 Ω·m | |
200.0 °C | 6.47E-7 Ω·m | |
300.0 °C | 7.27E-7 Ω·m | |
400.0 °C | 8.09E-7 Ω·m | |
500.0 °C | 8.9E-7 Ω·m | |
600.0 °C | 9.72E-7 Ω·m | |
700.0 °C | 1.06E-6 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Aluminium | 0.04 % |
Carbon | 0.08 - 0.15 % |
Chromium | 8 - 10 % |
Copper | 0.3 % |
Manganese | 0.3 - 0.6 % |
Molybdenum | 0.9 - 1.1 % |
Phosphorus | 0.03 % |
Silicon | 0.25 - 1 % |
Sulfur | 0.01 - 0.02 % |
Metal
- SEW 385 Ni42 Soft-Annealed Alloy (+A) – Low-Expansion, High-Performance Material
- SEW 385 Grade Ni46 Soft‑Annealed Alloy (+A) – High‑Performance Thermal Expansion Solution
- EN 10216-2 Grade 8MoB5-4 (Normalized/Normalized Formed +N): High‑Temperature Seamless Tubes for Boilers, Pipelines & Pressure Vessels
- EN 10250-4 Grade X4CrNiMo16-5-1 Soft Annealed Stainless Steel (+A) – High Corrosion Resistance & Low‑Temperature Performance
- DIN 17851 TiAl5Fe2.5 Annealed – High Strength, Corrosion Resistance & Biocompatibility
- DIN 17460 Grade X5NiCrAlTi31-20 – Solution Annealed Steel for High‑Temperature Applications
- EN 10216-2 X12CrMo91 Soft Annealed Steel – High-Performance Material for Hydrogenation & Petroleum Applications
- WL 3.1754 T6 Alloy – Premium Material for Gearboxes & Air Inlet Systems
- EN 10216-2 Grade St 45.8: High‑Temperature Normalized Tube Steel (+N) for Seamless Tubes
- UGI® 202N – Grade 1 Annealed: Premium High‑Manganese, Amagnetic Stainless Steel for Cryogenic Applications