DIN 17743 NiCu30Al: High-Temperature, Creep-Resistant Alloy for Corrosion-Resistant Applications
The creep-resistant Ni-Cu-wrought alloy NiCu30Al (K-Monel) is used in form of bars and forged pieces for high corrosion resistant and highest strength parts up to 450°C.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 8.46 g/cm³ |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | 20.0 °C | 178.54 GPa |
100.0 °C | 174.62 GPa | |
200.0 °C | 170.69 GPa | |
300.0 °C | 165.79 GPa | |
400.0 °C | 159.9 GPa | |
500.0 °C | 153.04 GPa | |
Elongation | -80.0 °C | 18 % |
20.0 °C | 17 - 23 % | |
100.0 °C | 23 % | |
200.0 °C | 23 % | |
300.0 °C | 23 % | |
400.0 °C | 12 % | |
500.0 °C | 4.5 % | |
600.0 °C | 1.5 % | |
700.0 °C | 3.5 % | |
Hardness, Brinell | 20.0 °C | 265 [-] |
Tensile strength | -80.0 °C | 1177 MPa |
20.0 °C | 962 - 1079 MPa | |
100.0 °C | 1030 MPa | |
200.0 °C | 1020 MPa | |
300.0 °C | 1010 MPa | |
400.0 °C | 903 MPa | |
500.0 °C | 726 MPa | |
600.0 °C | 589 MPa | |
700.0 °C | 461 MPa | |
Yield strength Rp0.2 | -80.0 °C | 785 MPa |
20.0 °C | 687 - 755 MPa | |
100.0 °C | 736 MPa | |
200.0 °C | 716 MPa | |
300.0 °C | 716 MPa | |
400.0 °C | 716 MPa | |
500.0 °C | 677 MPa | |
600.0 °C | 579 MPa | |
700.0 °C | 441 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | 100.0 °C | 1.4E-5 1/K | |
300.0 °C | 1.5E-5 1/K | ||
600.0 °C | 1.6E-5 1/K | ||
Max service temperature, long | 0 - 450 °C | ||
Melting point | 1170 - 1365 °C | Typical for Nickel Copper Alloy | |
Specific heat capacity | 20.0 °C | 427 J/(kg·K) | |
100.0 °C | 427 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 18 W/(m·K) | |
100.0 °C | 18 W/(m·K) | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical conductivity | 20.0 °C | 1.72E+6 S/m |
Electrical resistivity | 20.0 °C | 5.47E-7 Ω·m |
Chemical properties
| Property | Value |
|---|---|
Aluminium | 2 - 4 % |
Carbon | 0.25 % |
Cobalt | 1 % |
Copper | 27 - 34 % |
Iron | 2 % |
Manganese | 1.5 % |
Silicon | 1 % |
Sulfur | 0.01 % |
Titanium | 0.25 - 1 % |
Metal
- DIN 1725-2 Grade G-AlSi7Mg T6 Aluminium Alloy – Specifications & Properties
- DIN 5512-3 Grade X2CrNi12 Steel – High-Performance Rail Vehicle Material
- DIN 17864 TiAl6Zr5Mo0.5Si: Artificially Aged High‑Temperature Alloy
- DIN 17851 TiAl6Sn2Zr4Mo2Si: High-Strength, Artificially Aged Titanium Alloy
- DIN 17851 TiAl6V6Sn2 – Premium High-Strength, Corrosion-Resistant Titanium Alloy
- DIN 17743 LC-NiCu30Fe – Soft Annealed, Low‑Carbon, Corrosion‑Resistant Steel
- DIN 1614-1 Grade St 22: Premium Cold-Rolled Steel for Industrial Applications
- DIN 1614-1 Grade St 24: Premium Cold‑Rolled Steel Sheet & Strip
- DIN 17851 Grade TiAl6V4: Premium Artificially Aged Titanium Alloy – High Strength & Toughness
- DIN 17743 NiCu30Fe Soft-Annealed Alloy (+A) – Technical Standards & Applications