EN 10095 X18CrN28 Soft Annealed Steel – High Sulfureous Gas & Oil Ash Resistance
Ferritic chrome steel of high resistance to sulfureous gases. Heat-resistance in air up to 1100°C (highest application temp.). Application for recuperators in corrosive flue gas of carbon and heavy oil. Very high resistance to oil ash corrosion as well as to fused lead and tin.
Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.7 g/cm³ |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | 20.0 °C | 209.6 GPa |
95.0 °C | 205.46 GPa | |
150.0 °C | 202.71 GPa | |
205.0 °C | 198.57 GPa | |
260.0 °C | 195.12 GPa | |
315.0 °C | 190.99 GPa | |
370.0 °C | 185.47 GPa | |
425.0 °C | 179.26 GPa | |
Elongation | 20.0 °C | 15 % |
Elongation A80 | 20.0 °C | 13 % |
Hardness, Brinell | 20.0 °C | 212 [-] |
Poisson's ratio | 20.0 °C | 0.28 [-] |
95.0 °C | 0.27 [-] | |
150.0 °C | 0.29 [-] | |
205.0 °C | 0.29 [-] | |
260.0 °C | 0.3 [-] | |
315.0 °C | 0.29 [-] | |
370.0 °C | 0.29 [-] | |
425.0 °C | 0.3 [-] | |
Shear modulus | 20.0 °C | 82.05 GPa |
95.0 °C | 80.67 GPa | |
150.0 °C | 78.6 GPa | |
205.0 °C | 77.22 GPa | |
260.0 °C | 75.15 GPa | |
315.0 °C | 73.77 GPa | |
370.0 °C | 71.71 GPa | |
425.0 °C | 68.95 GPa | |
Tensile strength | 20.0 °C | 500 - 700 MPa |
Yield strength Rp0.2 | 20.0 °C | 280 MPa |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | 200.0 °C | 1E-5 1/K | |
400.0 °C | 1.1E-5 1/K | ||
600.0 °C | 1.15E-5 1/K | ||
800.0 °C | 1.2E-5 1/K | ||
1000.0 °C | 1.3E-5 1/K | ||
Max service temperature, long | 0 - 1000 °C | ||
Melting point | 1425 - 1530 °C | Typical for Ferritic Stainless Steel | |
Specific heat capacity | 20.0 °C | 500 J/(kg·K) | |
Thermal conductivity | 20.0 °C | 17 W/(m·K) | |
500.0 °C | 23 W/(m·K) | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 7E-7 Ω·m |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.15 - 0.2 % |
Chromium | 26 - 29 % |
Manganese | 1 % |
Nitrogen | 0.15 - 0.25 % |
Phosphorus | 0.04 % |
Silicon | 1 % |
Sulfur | 0.015 % |
Metal
- EN 10088-1 X70CrMo15: Soft Annealed Grade for Cutting Tools & Industrial Applications
- X105CrMo17 Soft Annealed Steel (EN 10088-1) – High Hardening & Wear Resistance
- EN 10083-2 Grade C50R Soft Annealed Steel (+A) – High Strength & Workability
- EN 10095 NiCr22Mo9Nb Soft‑Annealed Alloy (+A) – High‑Temperature Corrosion Resistance
- EN 10095 NiCr15Fe Soft Annealed (+A) – High-Temperature, Corrosion-Resistant Alloy
- EN 10095 X3CrAlTi18-2 Soft-Annealed Stainless Steel (+A) – High‑Temperature Performance to 1000 °C
- EN 10095 X10CrAlSi13 Heat‑Resistant Steel – Soft Annealed Grade (+A)
- EN 10095 X10CrAlSi18 Soft-Annealed Steel – High-Temperature Resistant Grade (+A)
- EN 10095 X10CrAlSi25 Soft Annealed Steel – High-Temperature Performance
- EN 10095 Grade X10CrAlSi7 Soft Annealed (+A) – High‑Temperature Resistant Chrome Steel