EN 10088-1 X50CrMoV15 Soft-Annealed Steel: High Strength & Abrasion Resistance

Material X50CrMoV15 is comparable to X 45 CrMoV 15 acc. to DIN 17440:1985-07. Hardenable steel of high strength and high abrasion resistance for all kinds of cutting tools, especially for partial hardened cutting tools, for ball bearing balls, wear resistant components, controlling and pump parts. Resistant to water and steam in hardened condition. Higher resistance than 1.4034 and 1.4110. Insufficient corrosion resistance in annealed or high tempered condition.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.56 - 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

215 - 218 GPa

100.0 °C

212 - 213 GPa

200.0 °C

205 - 206 GPa

300.0 °C

198 - 200 GPa

400.0 °C

190 GPa

500.0 °C

180 GPa

600.0 °C

167 GPa

700.0 °C

150 GPa

Elongation

20.0 °C

12 %

Elongation A80

20.0 °C

12 %

Hardness, Brinell

20.0 °C

280 [-]

Hardness, Rockwell B

20.0 °C

100 [-]

Hardness, Vickers

20.0 °C

280 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Typical for Martensitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Typical for Martensitic Stainless Steel

Tensile strength

20.0 °C

850 - 900 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

9.9E-6 1/K

100.0 °C

1.03E-5 - 1.05E-5 1/K

200.0 °C

1.08E-5 - 1.1E-5 1/K

300.0 °C

1.1E-5 - 1.12E-5 1/K

400.0 °C

1.15E-5 - 1.16E-5 1/K

500.0 °C

1.19E-5 1/K

600.0 °C

1.21E-5 1/K

700.0 °C

1.24E-5 1/K

800.0 °C

1.29E-5 1/K

Melting point

1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

450 - 460 J/(kg·K)

100.0 °C

482 J/(kg·K)

200.0 °C

506 J/(kg·K)

300.0 °C

525 J/(kg·K)

400.0 °C

547 J/(kg·K)

500.0 °C

576 J/(kg·K)

600.0 °C

616 J/(kg·K)

Thermal conductivity

20.0 °C

16 - 30 W/(m·K)

100.0 °C

17.2 W/(m·K)

200.0 °C

18.6 W/(m·K)

300.0 °C

20 W/(m·K)

400.0 °C

21.2 W/(m·K)

500.0 °C

22.3 W/(m·K)

600.0 °C

23.3 W/(m·K)

700.0 °C

24.1 W/(m·K)

800.0 °C

25.5 W/(m·K)

900.0 °C

26.9 W/(m·K)

1000.0 °C

28.3 W/(m·K)

Thermal diffusivity

20.0 °C

4.7 mm²/s

100.0 °C

4.5 mm²/s

200.0 °C

4.5 mm²/s

300.0 °C

4.6 mm²/s

400.0 °C

4.4 mm²/s

500.0 °C

4.1 mm²/s

600.0 °C

3.6 mm²/s

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6.5E-7 - 9.06E-7 Ω·m

100.0 °C

9.42E-7 Ω·m

200.0 °C

9.87E-7 Ω·m

300.0 °C

1.03E-6 Ω·m

400.0 °C

1.08E-6 Ω·m

500.0 °C

1.12E-6 Ω·m

600.0 °C

1.18E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

1000.0 °C

1.27E-6 Ω·m

Chemical properties

PropertyValue

Carbon

0.45 - 0.55 %

Chromium

14 - 15 %

Manganese

1 %

Molybdenum

0.5 - 0.8 %

Phosphorus

0.04 %

Silicon

1 %

Sulfur

0.015 %

Vanadium

0.1 - 0.2 %


Metal

  1. EN 10088-1 X70CrMo15: Soft Annealed Grade for Cutting Tools & Industrial Applications
  2. X105CrMo17 Soft Annealed Steel (EN 10088-1) – High Hardening & Wear Resistance
  3. EN 10088-1 Grade X90CrMoV18 – Soft Annealed Steel for High‑Performance Cutting Tools
  4. EN 10088‑1 Grade X2CrMoTiS18‑2 Soft‑Annealed Steel (+A) – Premium Ferritic Properties
  5. EN 10088-1 Grade X2CrMoTi29-4 Soft-Annealed Steel for Cold-Rolled Strips
  6. EN 10088-1 Grade X2CrAlTi18-2 Soft-Annealed Steel – Superior Corrosion Resistance & Mechanical Performance
  7. EN 10088-1 X6CrNi17-1 Soft‑Annealed Steel (+A) – High Corrosion Resistance & Strength
  8. EN 10088‑1 X6CrNiTi12 Soft‑Annealed Steel – Grade X6CrNiTi12 (+A) – Specifications & Properties
  9. EN 10088-1 X2CrMoTi17-1 Soft Annealed Steel – Superior Formability for Appliances & Pipes
  10. EN 10088-1 Grade X2CrNbZr17 Soft Annealed Steel (+A) – Superior Corrosion & Heat Resistance