The austenitic steel X6CrNiTi18-10 is available in the solution annealed condition. Welded circular tubes of this steel are used for compression load and for corrosive load at room temperature, low temperatures and elevated temperatures. The material is resistant to intercrystalline corrosion (up to 400 °C) also in the welded condition.
Additional services: To ensure our customers' processes and/or products attain – and even exceed – their performance expectations, we offer a wide range of services within both the technical area and delivery logistics. Our technical services include: • Material consultations through our worldwide sales network • Advice in process optimization based on an in-depth applications knowledge • Joint new product development supported by our extensive R&D program View product groups and servicesUGITECH
MANUFACTURER
Information and services
Additional services: https://eservices.ugitech.com/Properties
General
| Property | Temperature | Value |
|---|---|---|
Density | 20.0 °C | 7.9 - 7.93 g/cm³ |
Mechanical
| Property | Temperature | Value |
|---|---|---|
Elastic modulus | -100.0 °C | 206 GPa |
20.0 °C | 196 - 200 GPa | |
95.0 °C | 193.05 GPa | |
100.0 °C | 190 - 194 GPa | |
150.0 °C | 188.23 GPa | |
200.0 °C | 182 - 186 GPa | |
205.0 °C | 182.71 GPa | |
260.0 °C | 177.88 GPa | |
300.0 °C | 174 - 179 GPa | |
315.0 °C | 174.44 GPa | |
370.0 °C | 168.92 GPa | |
400.0 °C | 166 - 172 GPa | |
425.0 °C | 164.1 GPa | |
485.0 °C | 159.96 GPa | |
500.0 °C | 158 - 165 GPa | |
540.0 °C | 155.13 GPa | |
595.0 °C | 151 GPa | |
600.0 °C | 150 GPa | |
650.0 °C | 146.17 GPa | |
700.0 °C | 142 GPa | |
705.0 °C | 140.65 GPa | |
760.0 °C | 135.83 GPa | |
800.0 °C | 134 GPa | |
815.0 °C | 131.69 GPa | |
900.0 °C | 127 GPa | |
1000.0 °C | 120 GPa | |
Elongation | 20.0 °C | 35 % |
Elongation, transverse | 20.0 °C | 30 % |
Poisson's ratio | 20.0 °C | 0.29 [-] |
95.0 °C | 0.3 [-] | |
150.0 °C | 0.29 [-] | |
205.0 °C | 0.29 [-] | |
260.0 °C | 0.3 [-] | |
315.0 °C | 0.3 [-] | |
370.0 °C | 0.3 [-] | |
425.0 °C | 0.31 [-] | |
485.0 °C | 0.32 [-] | |
540.0 °C | 0.32 [-] | |
595.0 °C | 0.34 [-] | |
650.0 °C | 0.34 [-] | |
705.0 °C | 0.33 [-] | |
760.0 °C | 0.33 [-] | |
815.0 °C | 0.35 [-] | |
Shear modulus | 20.0 °C | 77.22 GPa |
95.0 °C | 74.46 GPa | |
150.0 °C | 73.08 GPa | |
205.0 °C | 71.02 GPa | |
260.0 °C | 68.26 GPa | |
315.0 °C | 66.88 GPa | |
370.0 °C | 64.81 GPa | |
425.0 °C | 62.74 GPa | |
485.0 °C | 60.67 GPa | |
540.0 °C | 58.61 GPa | |
595.0 °C | 56.54 GPa | |
650.0 °C | 54.47 GPa | |
705.0 °C | 53.09 GPa | |
760.0 °C | 51.02 GPa | |
815.0 °C | 48.95 GPa | |
Tensile strength | 20.0 °C | 500 - 730 MPa |
Tensile strength, transverse | 20.0 °C | 500 - 730 MPa |
Yield strength Rp0.2 | 20.0 °C | 200 MPa |
50.0 °C | 162 - 190 MPa | |
100.0 °C | 147 - 176 MPa | |
150.0 °C | 132 - 167 MPa | |
200.0 °C | 118 - 157 MPa | |
250.0 °C | 108 - 147 MPa | |
300.0 °C | 100 - 136 MPa | |
350.0 °C | 94 - 130 MPa | |
400.0 °C | 89 - 125 MPa | |
450.0 °C | 85 - 121 MPa | |
500.0 °C | 81 - 119 MPa | |
550.0 °C | 80 - 118 MPa | |
Yield strength Rp0.2, transverse | 20.0 °C | 200 MPa |
Yield strength Rp1.0 | 20.0 °C | 235 MPa |
50.0 °C | 201 - 222 MPa | |
100.0 °C | 181 - 208 MPa | |
150.0 °C | 162 - 195 MPa | |
200.0 °C | 147 - 185 MPa | |
250.0 °C | 137 - 175 MPa | |
300.0 °C | 127 - 167 MPa | |
350.0 °C | 121 - 161 MPa | |
400.0 °C | 116 - 156 MPa | |
450.0 °C | 112 - 152 MPa | |
500.0 °C | 109 - 149 MPa | |
550.0 °C | 108 - 147 MPa | |
Thermal
| Property | Temperature | Value | Comment |
|---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K | ||
Melting point | 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 14.3 - 15 W/(m·K) | |
100.0 °C | 15.8 W/(m·K) | ||
200.0 °C | 17.5 W/(m·K) | ||
300.0 °C | 19 W/(m·K) | ||
400.0 °C | 20.5 W/(m·K) | ||
500.0 °C | 21.9 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) | ||
700.0 °C | 24.6 W/(m·K) | ||
800.0 °C | 26 W/(m·K) | ||
900.0 °C | 27.4 W/(m·K) | ||
1000.0 °C | 28.8 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.8 mm²/s | |
100.0 °C | 4 mm²/s | ||
200.0 °C | 4.2 mm²/s | ||
300.0 °C | 4.6 mm²/s | ||
400.0 °C | 4.8 mm²/s | ||
500.0 °C | 4.9 mm²/s | ||
600.0 °C | 5 mm²/s | ||
700.0 °C | 5.3 mm²/s | ||
800.0 °C | 5.6 mm²/s | ||
900.0 °C | 5.9 mm²/s | ||
1000.0 °C | 6 mm²/s | ||
Electrical
| Property | Temperature | Value |
|---|---|---|
Electrical resistivity | 20.0 °C | 7.1E-7 - 7.3E-7 Ω·m |
100.0 °C | 7.76E-7 Ω·m | |
200.0 °C | 8.49E-7 Ω·m | |
300.0 °C | 9.14E-7 Ω·m | |
400.0 °C | 9.71E-7 Ω·m | |
500.0 °C | 1.02E-6 Ω·m | |
600.0 °C | 1.07E-6 Ω·m | |
700.0 °C | 1.1E-6 Ω·m | |
800.0 °C | 1.14E-6 Ω·m | |
900.0 °C | 1.17E-6 Ω·m | |
1000.0 °C | 1.19E-6 Ω·m | |
Chemical properties
| Property | Value |
|---|---|
Carbon | 0.08 % |
Chromium | 17 - 19 % |
Manganese | 2 % |
Nickel | 9 - 12 % |
Phosphorus | 0.05 % |
Silicon | 1 % |
Sulfur | 0.015 % |
Titanium | 0.7 % |
Metal
- EN 10222-5 X2CrNiMo18-14-3 Solution‑Annealed Grade for Corrosion‑Resistant Applications
- EN 10222-5 X6CrNiMoTi17-12-2 (Solution Annealed) – High Corrosion‑Resistant Stainless Steel
- EN 10222-5 X6CrNiTi18-10 – Solution Annealed & AT: Premium Corrosion‑Resistant Steel for Chemical & Food Applications
- EN 10250‑4 X6CrNiTi18‑10: Ti‑Stabilized, Solution‑Annealed Stainless Steel for High‑Performance Welding
- EN 10217-7 X5CrNi18-10 Austenitic Steel – Solution Annealed (+AT) for Corrosion Resistance
- EN 10217-7 Grade X6CrNiMoTi17-12-2 Solution-Annealed Steel – High‑Temperature Corrosion Resistance & Structural Strength
- EN 10217-7 X6CrNiTi18-10 Solution-Annealed Austenitic Steel – Corrosion-Resistant & High-Temperature Performance
- X2CrNiMo18-14-3 Austenitic Steel – Solution Annealed (EN 10217‑7) – Superior Corrosion & Temperature Resistance
- EN 10216-5 X6CrNiTi18-10 Solution-Annealed – Titanium‑Stabilized Stainless Steel with Superior Corrosion Resistance & Weldability
- EN 10028-7 X6CrNiTi18-10 Solution-Annealed Steel: High-Temp, Corrosion-Resistant, Pressure Vessel & Civil Engineering Grade